Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)

Laboratory rubber stoppers from a 1909 rubber factory's book of mixings: Pará rubber with ceresine wax, sulphur and magnesia, run out as a cord, cut to weight, pressed into moulds and cured. Source: Heil & Esch, The Manufacture of Rubber Goods (1909), mixing No. 34 (p. 108) and the stopper method (p. 135). They give no cure time or temperature. Using smoked ball rubber as their Pará, and the mill, clamps and steam vessel, are ours. Picture: their page of mixings.
មធ្យម
1 day

ការណែនាំ

1

Weigh mixing No. 34

Weigh out 10,000 g Pará rubber, 2,000 g ceresine, 1,000 g sulphur and 100 g calcined magnesia (magnesia usta).

សម្ភារៈសម្រាប់ជំហាននេះ៖

ដុំកៅស៊ូមូលឆ្អើរដុំកៅស៊ូមូលឆ្អើរ10000 ក្រ
ក្រមួនសេរ៉េស៊ីនក្រមួនសេរ៉េស៊ីន2000 ក្រ
ម្សៅស្ពាន់ធ័រម្សៅស្ពាន់ធ័រ1000 ក្រ
ម៉ាញេស្យូមអុកស៊ីតម៉ាញេស្យូមអុកស៊ីត100 ក្រ

ឧបករណ៍ដែលត្រូវការ៖

ជញ្ជីងចានពីរជញ្ជីងចានពីរ
2

Mix on the rolls

Work the rubber on the mixing rolls and work the ceresine, sulphur and magnesia into it until the mixing is even.

ឧបករណ៍ដែលត្រូវការ៖

ម៉ាស៊ីនកិនកៅស៊ូរ៉ូឡូពីរម៉ាស៊ីនកិនកៅស៊ូរ៉ូឡូពីរ
3

Run a cord on the tube machine

Run the mixing through the tube machine as a cord of a size to suit the stoppers. It must be free from air bubbles, or the stoppers will be faulty after curing.

ឧបករណ៍ដែលត្រូវការ៖

ម៉ាស៊ីនបំពង់កៅស៊ូម៉ាស៊ីនបំពង់កៅស៊ូ
4

Cut pieces to weight

Cut the cord into pieces of the exact weight of one stopper plus 2 or 3 per cent, for what squeezes out of the mould.

ឧបករណ៍ដែលត្រូវការ៖

កាំបិតសិប្បកម្មកាំបិតសិប្បកម្ម
ជញ្ជីងចានពីរជញ្ជីងចានពីរ
5

Press into moulds and clamp

Press each piece into a mould and clamp the small moulds very tightly in iron clips.

ឧបករណ៍ដែលត្រូវការ៖

ពុម្ពវ៉ុលកាណៃស៍ពុម្ពវ៉ុលកាណៃស៍
ដង្កៀបរាងអក្សរ Cដង្កៀបរាងអក្សរ C
6

Cure in steam

Cure the clamped moulds in a steam heater (Heil & Esch also name the sulphur bath). They give no time or temperature for stoppers; then open the moulds and take out the stoppers.

ឧបករណ៍ដែលត្រូវការ៖

អូតូក្លាវលើតុអូតូក្លាវលើតុ
ពុម្ពវ៉ុលកាណៃស៍ពុម្ពវ៉ុលកាណៃស៍

សម្ភារៈ

4

ឧបករណ៍ចាំបាច់

7

ប្លង់ពាក់ព័ន្ធ

ប្លង់ទាំងនេះចែករំលែកចំណេះដឹង — បច្ចេកទេស សម្ភារៈ ឬគោលការណ៍

CC0 សាធារណៈ

ប្លង់នេះត្រូវបានចេញផ្សាយក្រោម CC0។ អ្នកមានសិទ្ធិចម្លង កែប្រែ ចែកចាយ និងប្រើប្រាស់ដោយមិនចាំបាច់សុំអនុញ្ញាត។

គាំទ្រអ្នកបង្កើតដោយទិញផលិតផលតាមរយៈប្លង់របស់ពួកគេ ដែលពួកគេទទួលបាន កម្រៃជើងសារអ្នកបង្កើត កំណត់ដោយអ្នកលក់ ឬបង្កើតកំណែថ្មីនៃប្លង់នេះ ហើយបញ្ចូលជាការតភ្ជាប់ក្នុងប្លង់របស់អ្នកដើម្បីចែករំលែកចំណូល។

ការពិភាក្សា

(0)

ចូល ដើម្បីចូលរួមពិភាក្សា

កំពុងផ្ទុកមតិ...