Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
Ed

បង្កើតដោយ

Ed

28. តុលា 2026FI
3
0
0
0
0

Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)

A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1350 °C and fired with the paste at 800 °C, the disc measured a C-value of 90 at 1 mA and a nonlinearity exponent n of 7.3. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
កម្រិតខ្ពស់
2 days

ការណែនាំ

1

Press pure zinc oxide at 340 kg/cm²

Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.

សម្ភារៈសម្រាប់ជំហាននេះ៖

ម្សៅស័ង្កសីអុកស៊ីតម្សៅស័ង្កសីអុកស៊ីត1 as required

ឧបករណ៍ដែលត្រូវការ៖

ជញ្ជីងចានពីរជញ្ជីងចានពីរ
ម៉ាស៊ីនសង្កត់អ៊ីដ្រូលិកម៉ាស៊ីនសង្កត់អ៊ីដ្រូលិក
ពុម្ពសង្កត់ថាសពុម្ពសង្កត់ថាស
ខ្នាតវ៉ែនញ្ញេខ្នាតវ៉ែនញ្ញេ
2

Sinter 1 hour at 1350 °C and cool

Heat the pressed disc for 1 hour at 1350 °C, then let it cool to room temperature.

ឧបករណ៍ដែលត្រូវការ៖

ឡដុតមូហ្វលឡដុតមូហ្វល
3

Lap both faces

Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.

ឧបករណ៍ដែលត្រូវការ៖

គ្រាប់ស៊ីលីកូនកាបួតគ្រាប់ស៊ីលីកូនកាបួត
ខ្នាតវ៉ែនញ្ញេខ្នាតវ៉ែនញ្ញេ
4

Coat with bismuth oxide paste and fire at 800 °C

Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.

សម្ភារៈសម្រាប់ជំហាននេះ៖

អុកស៊ីតប៊ីស្មុតអុកស៊ីតប៊ីស្មុត1 as required

ឧបករណ៍ដែលត្រូវការ៖

អេប៉ុកស៊ីរេស៊ីនអេប៉ុកស៊ីរេស៊ីន
n-ប៊ូតាណុលn-ប៊ូតាណុល
ឡដុតមូហ្វលឡដុតមូហ្វល
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.

សម្ភារៈសម្រាប់ជំហាននេះ៖

ដុំអាលុយមីញ៉ូមដុំអាលុយមីញ៉ូម1 as required
ថ្នាំលាបប្រាក់ចម្លងចរន្តថ្នាំលាបប្រាក់ចម្លងចរន្ត1 as required
ខ្សែស្ពាន់ខ្សែស្ពាន់2 ដុំ

ឧបករណ៍ដែលត្រូវការ៖

វិធីបាញ់លោហៈដែលមិនស្គាល់វិធីបាញ់លោហៈដែលមិនស្គាល់
ខ្នាតវ៉ែនញ្ញេខ្នាតវ៉ែនញ្ញេ

សម្ភារៈ

5

ឧបករណ៍ចាំបាច់

9

ប្លង់ពាក់ព័ន្ធ

ប្លង់ទាំងនេះចែករំលែកចំណេះដឹង — បច្ចេកទេស សម្ភារៈ ឬគោលការណ៍

CC0 សាធារណៈ

ប្លង់នេះត្រូវបានចេញផ្សាយក្រោម CC0។ អ្នកមានសិទ្ធិចម្លង កែប្រែ ចែកចាយ និងប្រើប្រាស់ដោយមិនចាំបាច់សុំអនុញ្ញាត។

គាំទ្រអ្នកបង្កើតដោយទិញផលិតផលតាមរយៈប្លង់របស់ពួកគេ ដែលពួកគេទទួលបាន កម្រៃជើងសារអ្នកបង្កើត កំណត់ដោយអ្នកលក់ ឬបង្កើតកំណែថ្មីនៃប្លង់នេះ ហើយបញ្ចូលជាការតភ្ជាប់ក្នុងប្លង់របស់អ្នកដើម្បីចែករំលែកចំណូល។

ការពិភាក្សា

(0)

ចូល ដើម្បីចូលរួមពិភាក្សា

កំពុងផ្ទុកមតិ...