Adhesion: Four Tests, and Three of Them Destroy the Part
Charlie

작성자

Charlie

24. 9월 2026DE
21
0
0
0
0

Adhesion: Four Tests, and Three of Them Destroy the Part

A plated part that looks perfect and a plated part that will peel next month are indistinguishable by eye. Adhesion has to be tested, and every worthwhile test destroys the piece it is performed on. So the standard practice is to plate a **test coupon** alongside the real work, from the same batch, through the same baths, and to destroy that instead. A coupon costs a scrap of steel and answers the only question that matters. The tests are simple, they need no equipment, and the failure modes each point at a different mistake earlier in the process.
중급
2 hours

안내

1

The bend test and the burnish test

**The bend test.** Bend the coupon through 180 degrees over a mandrel of a few times its thickness, then examine the outside of the bend under magnification. A well-adhered coating **cracks with the substrate** — it may craze, but the pieces stay attached, because the coating and the metal are failing together. A poorly adhered coating **lifts, flakes or peels away from the bend**, often in a sheet. That is a clean separation at the interface, and it means the surface was not clean. **The burnish test.** Rub a small area briskly with a smooth hard tool — the back of a knife, a burnisher — for fifteen seconds. A well-adhered coating polishes. A poorly adhered one blisters, because the friction works it loose from underneath. **The file test.** File across the edge of the coupon at 45 degrees, from the substrate towards the coating. A good coating is cut through cleanly; a bad one lifts ahead of the file. **Look at the WAY it failed.** A coating that lifts in large sheets with a shiny back was on a greasy surface. One that lifts in small flakes with a dull grey back was on an oxidised one. The fracture surface names the cause.

이 단계의 재료:

연강판연강판2 개
니켈판니켈판1 개

필요한 도구:

확대 루페확대 루페
2

Thermal shock, which finds what the others miss

**Heat the part and quench it.** The coating and the substrate expand by different amounts, so a sudden temperature change puts a large shear stress directly on the interface — which is exactly what an adhesion test wants to do. Typical: 150 to 300 C for an hour, depending on the substrate, then straight into cold water. Blistering or peeling afterwards is a fail. **It is the most searching of the tests**, because it stresses the whole area at once rather than one line, and it finds marginal adhesion that a bend test passes. **It doubles as the hydrogen bake.** Heating plated high-strength steel to 190 to 220 C for several hours drives dissolved hydrogen out before it can cause delayed brittle fracture, and it must be done within hours of plating. A part that both bakes and survives the quench has answered two questions. **Do not thermal-shock a part that has been hardened**, unless the temperature is safely below its tempering temperature. The test would ruin the part in a different way. **Record which test was used** alongside the result. "Passed adhesion" means nothing without it, in the same way that a purity figure means nothing without its method.

이 단계의 재료:

연강판연강판2 개

필요한 도구:

실험용 온도계실험용 온도계
붕규산 비커붕규산 비커
내화학 장갑내화학 장갑
3

Why adhesion fails, in order of likelihood

**Contamination.** Oil, grease, a fingerprint, polishing compound, or drag-in from a previous bath. This is the great majority of failures, and the water-break test would have caught it. **Oxide.** The part was pickled, then stood in air, then plated. A clean steel surface re-oxidises visibly in minutes and invisibly in seconds. **Passivity.** Some metals — stainless steel, aluminium, titanium, chromium — carry an oxide film that re-forms faster than it can be removed. They need a specific activation step: a **Wood's nickel strike** for stainless, a zincate for aluminium. Plating them directly always fails, however clean they are. **Interrupted current.** If the current stops mid-plate and then restarts, the surface passivates in the gap and the second layer does not bond to the first. A bath that has lost power is stripped and restarted, not resumed. **Internal stress.** A highly stressed deposit — bright nickel with too much brightener, or chromium, which is always in tension — pulls itself off a marginal bond. It can peel weeks later with nothing else having changed. **Dissimilar expansion.** A thick hard coating on a substrate with a very different expansion coefficient, in service across a temperature range. The first two account for most of it, and both are preparation.

이 단계의 재료:

연강판연강판1 개
니켈판니켈판1 개

필요한 도구:

확대 루페확대 루페
4

Stripping and starting again

A failed coating has to come off completely before another can go on, and a partially stripped part plates worse than a bare one. **Chemical stripping** is the usual route and it is specific to the pair of metals. The requirement is a solution that dissolves the coating and does not attack the substrate — which is exactly the opposite of the plating chemistry, and is why a strip for nickel-on-steel is not a strip for nickel-on-brass. **Reverse-current stripping** makes the part the anode and dissolves the coating off electrochemically. Controllable, and it stops when the coating is gone if the solution is chosen so the substrate passivates. **Mechanical stripping** — blasting, grinding — always removes some substrate and changes the dimensions. It is the last resort on a precision part and the first choice on a rough one. **Then start from the beginning.** A stripped part goes back through mechanical preparation, degreasing and pickling, not straight into the plating tank. The stripping solution is itself contamination. **Consider whether it is worth it.** Stripping and replating a small part often costs more than the part. The decision is easier with a test coupon, because the failure is discovered on the coupon rather than after the part is assembled into something.

이 단계의 재료:

10 % 묽은 염산10 % 묽은 염산1 개
연강판연강판1 개

필요한 도구:

붕규산 비커붕규산 비커
가변 실험용 전원 장치가변 실험용 전원 장치
내화학 장갑내화학 장갑
화학물질 비산 보안경화학물질 비산 보안경

재료

3

필요 도구

6

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...