Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)
Charlie

작성자

Charlie

28. 10월 2026DE
4
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Part of the Barium Replaced by Calcium (Went, Philips 1956, Ex. 21)

A ceramic magnet in which part of the barium is replaced by calcium: 0.06 mol barium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, milled, fired in oxygen, milled again, pressed and passed quickly through a hot furnace. Went's rod held 1,660 gauss with a coercive force of 1,210 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 21. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
고급
2 days

안내

1

Weigh barium carbonate, chalk and iron oxide

Weigh 11.84 g barium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol) and 99.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

이 단계의 재료:

탄산바륨(독중석)탄산바륨(독중석)11.84 g
탄산칼슘(호분)탄산칼슘(호분)4.004 g
산화제이철산화제이철99.55 g

필요한 도구:

접시 저울접시 저울
고무장갑고무장갑
P100 방진 마스크P100 방진 마스크
2

Mill with alcohol 4 hours and dry

Grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
3

Presinter in oxygen at 1000 °C for 2 hours

Fire the dry powder in oxygen at 1000 °C for 2 hours (ours: a tube furnace fed from an oxygen cylinder).

필요한 도구:

관상로관상로
산소산소
고압 가스통고압 가스통
내열 장갑내열 장갑
4

Mill again 4 hours, dry, press at 1.5 t/cm²

Grind with alcohol in the ball mill for 4 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods).

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
유압 프레스유압 프레스
원판 압축 금형원판 압축 금형
5

Pass through a 1200 °C zone in 10 minutes

Sinter at 1200 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute, which is 10 minutes in the heat.

필요한 도구:

관상로관상로
내열 장갑내열 장갑
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

필요한 도구:

전자석전자석
나침반나침반

재료

3

필요 도구

14

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...