Extruded Polystyrene Foam
Carl Munters had shown that polystyrene heated with methyl chloride under pressure puffs into a closed-cell foam when let out of the vessel (US 2,023,204) - but only in small pieces; with larger outlets the mass collapsed into brittle, irregular lumps. Otis Ray McIntire at Dow found the fix: keep the mass BELOW the critical temperature of methyl chloride, about 143 °C, so the gas stays dissolved, and let its own evaporation cool the foam fast enough to freeze the cells.
**US 2,450,436**, "Manufacture of cellular thermoplastic products", McIntire, assigned to Dow Chemical, filed 26. July 1947, granted 5. October 1948. Its drawing is the pressure vessel with the bottom valve the foam flows out of. Dow sold the result as blue insulation board; the white bead foam of packaging is a later process.
**Methyl chloride is toxic; you start from foam board.** You build a hot-wire cutter, cut an insulated box, and measure how long it keeps ice.
초급
3 hours plus an ice test
안내
1
1
The cutter
The cutter
Base on two feet, a post and an arm; the wire runs from the arm tip down through the base to a spring underneath.
2
2
Build the frame
Build the frame
From 18 mm plywood cut a 300 x 300 mm base, two 300 x 40 mm feet, a 280 x 50 mm post and a 200 x 50 mm arm. Glue and screw the post to the back edge and the arm square on top.
이 단계의 재료:
합판1 개
나사못10 개
목공용 접착제20 ml필요한 도구:
손톱(핸드소)
무선 드릴
드라이버 세트
강철 자3
3
String the wire
String the wire
Drill 2 mm through the arm tip and the base directly below. Fix the wire to an eye bolt on top of the arm, run it down through the base, and tie it to a spring under the base so it stays taut when it expands hot. Check it is square to the table.
이 단계의 재료:
니크롬선 80/20, 0.64 mm1 미터
아이볼트1 개
압축 스프링 세트1 세트필요한 도구:
무선 드릴
케이스 드릴 비트 세트4
4
Power it
Power it
Clip leads to the wire at the arm and below the base. Set the bench supply to 1.5 V with a 4 A limit and raise it slowly (notebook) until the wire slides through a scrap cleanly. Ventilate.
필요한 도구:
가변 실험용 전원 장치
Alligator to Alligator Cables
N95 방진 마스크
투명 보안경5
5
Cut the box
Cut the box
From 25 mm foam board cut a base and lid 200 x 200 mm, two sides 200 x 150 mm and two 150 x 150 mm. Feed slowly - let the wire do the work. Tape the box together.
이 단계의 재료:
압출 발포 폴리스티렌 보드1 장
마스킹 테이프1 롤필요한 도구:
강철 자6
6
Weigh a cube
Weigh a cube
Cut a 50 mm cube from an offcut and weigh it for the notebook.
필요한 도구:
디지털 주방 저울7
7
The ice test
The ice test
Put 500 g of ice in a bag in the foam box and another 500 g in a cardboard box of the same size, side by side in the same room. Note the room temperature and check both every hour until the ice is gone.
이 단계의 재료:
얼음 조각1000 g
골판지 상자1 개필요한 도구:
디지털 주방 저울
실내 온도계8
8
Wire, density, heat leak
Wire, density, heat leak
Jupyter 노트북 불러오는 중…
9
9
History & Context
History & Context
**What the patent specifies:** polystyrene with methyl chloride dissolved under pressure below the gas's critical temperature, released through an outlet so evaporation expands and cools it into uniform closed cells, in blocks 2 inches thick or more. **Modern build (derived):** commercial extruded foam board, today made with other blowing agents.
The patent names its target plainly: blocks big enough to cut into insulating panels for refrigerators. Its limits: it melts at low heat, burns unless treated, dissolves in many solvents (and in some glues and paints), and breaks down in sunlight.

재료
10- 1 개플레이스홀더
- 10 개플레이스홀더
- 20 ml플레이스홀더
- 플레이스홀더
- 1 개플레이스홀더
- 1 세트플레이스홀더
- 플레이스홀더
- 1 롤플레이스홀더
- 1000 g플레이스홀더
- 1 개플레이스홀더
필요 도구
11- 플레이스홀더
- 1 vendor sell this, none ship to you yet플레이스홀더
- 플레이스홀더
- 플레이스홀더
- 플레이스홀더
- 플레이스홀더
- ₩49
- 플레이스홀더
- 플레이스홀더
- 플레이스홀더
- 플레이스홀더
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.