Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)
Charlie

작성자

Charlie

1. 11월 2026DE
7
0
0
0
0

Ferromolybdenum: Molybdic Oxide Smelted with Coke and Lime into Molten Steel in an Electric Arc Furnace (Brigham, US 4,160,661)

Technical molybdic oxide is fed in cans, with coke and lime, into a bath of molten steel in a 3000 kVA arc furnace. The electrodes stay in the slag, and the coke is trimmed after every charge unit so the metal keeps under 0.1 % carbon. Ferrosilicon and lime strip the slag, and the metal is shotted in running water. Result: from 5000 lb oxide, 3110 lb shot and pig of 54.1 % molybdenum, 0.06 % carbon, 43.1 % iron (Heat 4), using 1.94 kWh per lb of molybdenum. Source: Brigham, Sirianni and Garner, US patent 4,160,661 (1979), Example 2, Heat 4. Not given: how the shot was heated while drying overnight. Picture drawn by Youblob.
고급
1 day

안내

1

Melt the steel

In a three-phase 3000 kVA arc furnace with 8 in graphite electrodes, lined with magnesia brick and rammed basic refractory (about 60 % MgO), 5 ft 6 in across and 26 in deep below the tap hole, melt 812 lb steel plate with 80 lb burnt lime under full power. Lead the fume to a bag house.

이 단계의 재료:

연강판연강판812 파운드

필요한 도구:

생석회생석회
전기 아크로전기 아크로
흑연 전극흑연 전극
백하우스백하우스
2

Make up the charge units

While it melts, weigh out five charge units, each 1000 lb molybdic oxide (in cans of 37 lb oxide in a 2 lb steel can), 250 lb coke and 320 lb lime. For Heat 4 that was 5000 lb oxide, 1150 lb coke, 1600 lb lime and 1488 lb steel in plate and cans. Ours: metallurgical coke for the dried breeze coke.

이 단계의 재료:

공업용 산화몰리브덴공업용 산화몰리브덴5000 파운드
연강판연강판1488 파운드

필요한 도구:

야금용 코크스야금용 코크스
생석회생석회
산업용 판 저울산업용 판 저울
3

Smelt in the bath

When the bath is molten at about 1450 °C, add one can of oxide with equal shovels of coke and lime every 2 minutes, about 1 hour per unit. Use the 205 V tap so the electrodes dip only into the slag; hold the bath at most 1760 °C. About 1 kWh per lb of oxide.

필요한 도구:

삽삽
전기 아크로전기 아크로
4

Keep the carbon down

After every charge unit, dip a steel spoon into the bath and analyse the carbon (about 15 minutes); cut the coke so the metal stays below 0.1 % carbon.

필요한 도구:

야금용 코크스야금용 코크스
5

Strip the slag and tap

Add 200 lb ferrosilicon and 560 lb lime to strip the slag. Tip the furnace into a preheated 5000 lb ladle: the first ladle is mostly slag, the second mostly metal. Back-pour the slag into slag pots.

필요한 도구:

페로실리콘페로실리콘
생석회생석회
주조용 국자주조용 국자
6

Shot the metal

Pour the metal from the ladle into a second unlined 5000 lb ladle filled with running water from a 2 1/4 in fire hose, about 3000 lb a minute, from about 4 ft up; 2000 lb shots in 10 to 15 minutes. Dry the shot overnight at about 300 °F in 40 gallon drums. Ours: a drying oven.

필요한 도구:

주조용 국자주조용 국자
물물
건조 가마건조 가마

재료

2

필요 도구

11

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...