Barium Ferrite Disc Magnet: Example 4 Without the Orienting Field (Gorter, Philips 1956, Ex. 4 Comparison)
Charlie

작성자

Charlie

28. 10월 2026DE
11
0
0
0
0

Barium Ferrite Disc Magnet: Example 4 Without the Orienting Field (Gorter, Philips 1956, Ex. 4 Comparison)

Made as in Example 4 but without the first, orienting field. Gorter's comparison block held 2,150 gauss with a coercive force of 2,000 oersted and a (BH)max of 0.9 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 4. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
고급
3 days

안내

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

이 단계의 재료:

탄산바륨(독중석)탄산바륨(독중석)450 g
산화제이철산화제이철2000 g

필요한 도구:

접시 저울접시 저울
고무장갑고무장갑
P100 방진 마스크P100 방진 마스크
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

필요한 도구:

관상로관상로
뚜껑 달린 도가니(자기)뚜껑 달린 도가니(자기)
내열 장갑내열 장갑
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

필요한 도구:

폴리아세트산비닐폴리아세트산비닐
아세톤아세톤
접시 저울접시 저울
6

Mould without a first field

Put the suspension in a moulding die and remove the binder solution without any magnetic field. This is the patent's comparison block.

필요한 도구:

원판 압축 금형원판 압축 금형
유압 프레스유압 프레스
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

필요한 도구:

관상로관상로
전자석전자석
내열 장갑내열 장갑
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

필요한 도구:

관상로관상로
내열 장갑내열 장갑
9

Magnetise the block

Magnetise the block in a field. Without the orienting field it has no preferred direction. Ours: an electromagnet. Find the north face with a compass.

필요한 도구:

전자석전자석
나침반나침반

재료

2

필요 도구

15

이 블루프린트로 만드는 것

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...