Oriented Strontium Ferrite Disc Magnet: Agate-Milled, 10,000 Oersted Field (Gorter, Philips 1956, Ex. 8)
Charlie

작성자

Charlie

28. 10월 2026DE
8
0
0
0
0

Oriented Strontium Ferrite Disc Magnet: Agate-Milled, 10,000 Oersted Field (Gorter, Philips 1956, Ex. 8)

A strontium ferrite magnet oriented in a magnetic field: strontium carbonate and iron oxide milled, pre-fired 2 hours at 1000 °C, ground fine in an agate mill, then oriented, heated and sintered as in Example 4. In the principal direction it held 2,640 gauss with a coercive force of 2,825 oersted and a (BH)max of 1.63 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
고급
3 days

안내

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g strontium carbonate and 179 g ferric oxide.

이 단계의 재료:

탄산스트론튬탄산스트론튬29.5 g
산화제이철산화제이철179 g

필요한 도구:

접시 저울접시 저울
P100 방진 마스크P100 방진 마스크
2

Mill 15 hours with alcohol, dry

Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.

필요한 도구:

철 볼 밀철 볼 밀
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
3

Pre-fire 2 hours at 1000 °C in air

Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.

필요한 도구:

머플로머플로
뚜껑 달린 도가니(자기)뚜껑 달린 도가니(자기)
도가니 집게도가니 집게
내열 장갑내열 장갑
4

Grind 4 hours in an agate centrifugal mill

Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.

필요한 도구:

마노 원심 분쇄기마노 원심 분쇄기
에탄올 - 실험실 등급, 95 %에탄올 - 실험실 등급, 95 %
건조 가마건조 가마
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

필요한 도구:

폴리아세트산비닐폴리아세트산비닐
아세톤아세톤
접시 저울접시 저울
6

Orient in a 10000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.

필요한 도구:

원판 압축 금형원판 압축 금형
전자석전자석
유압 프레스유압 프레스
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

필요한 도구:

관상로관상로
전자석전자석
내열 장갑내열 장갑
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

필요한 도구:

관상로관상로
내열 장갑내열 장갑
9

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

필요한 도구:

전자석전자석
나침반나침반

재료

2

필요 도구

17

이 블루프린트로 만드는 것

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.