PLA Pellets: Purified Lactide Polymerised with a Trace of Litharge
PLA (polylactide) is the polymer of lactic acid, the stock for PLA filament. Schneider's du Pont patent (US 2,703,316, 1955) made a tough, clear polymer by heating very pure lactide with a trace of litharge in a closed, evacuated vessel: at 180 °C it was done in 6½ hours. Above 200 °C the polymer falls back to lactide. Extruding it and cutting the strand into pellets is our step.
The picture: our diagram.
고급
About 8 hours
안내
1
1
Charge lactide and litharge
Charge lactide and litharge
Weigh 10 parts of purified lactide (melting at 125 °C in the patent's example; it must melt at 120 °C or above) and 0.004 part litharge into the reaction vessel.
이 단계의 재료:
락티드10 parts필요한 도구:
산화납(밀타승)
접시 저울
가압 반응기
P100 방진 마스크2
2
Evacuate and close
Evacuate and close
Pump the air out of the vessel and close it.
필요한 도구:
진공 펌프
진공계
가압 반응기3
3
Heat 6½ hours at 180 °C
Heat 6½ hours at 180 °C
Heat at 180 °C for 6½ hours. Do not go above 200 °C, where the polymer turns back to lactide. The product is a clear, colourless polymer (the example's softened at about 82 °C).
필요한 도구:
건조 가마
실험용 온도계
가압 반응기4
4
Extrude and pelletise
Extrude and pelletise
Ours: take the polymer out, melt it through an extruder and cut the cooled strand into pellets.
필요한 도구:
플라스틱 압출기
펠리타이저
내열 장갑이 블루프린트로 만드는 것
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.