Russia Sheet Iron: Charcoal-Packed Sheets Hammered to a Mirror Polish (Jordan after Koulibine, 1867)
Forge

작성자

Forge

4. 11월 2026NO
5
0
0
0
0

Russia Sheet Iron: Charcoal-Packed Sheets Hammered to a Mirror Polish (Jordan after Koulibine, 1867)

The glossy blue-black Russia sheet iron, long a Russian secret, as the engineer Koulibine described it to Professor Jordan for the Paris Exhibition of 1867: charcoal iron is rolled into black sheets, then packed red-hot with powdered charcoal between them and hammered under a one-ton hammer, then polished cold under a second. The charcoal, shut in between the hot sheets without air, cements the surface: it takes a high polish and rusts less. Once cemented, a sheet must not go back into the heating furnace. Unknown: how the charcoal finery iron is made. The source does not give it. Source: 'Russia Sheet Iron', Scientific American Supplement No. 154 (1878), pp. 2448-2449, after Jordan's 1867 report. Picture: the article.
고급
Unknown

안내

1

Roll the blooms into leaves

Start from charcoal iron made in finery fires and brought into blooms about one inch thick. Heat the blooms to cherry heat and roll them into leaves. Ours: the furnace and the rolling mill; the source names neither.

이 단계의 재료:

목탄 정련철목탄 정련철1 blooms about 1 inch thick

필요한 도구:

반사로반사로
압연기압연기
대장간 집게대장간 집게
2

Roll the black sheets

Cut each leaf into pieces that match the weight of the sheets to be made. Pile the pieces on one another and roll them together until they are as thin as wanted. These are the black sheets.

필요한 도구:

판금 전단기판금 전단기
반사로반사로
압연기압연기
대장간 집게대장간 집게
3

Pack with charcoal

Heat a number of black sheets at a time to red heat and pile them one on another, sprinkling pulverized charcoal, a black impalpable powder, between each two. Two thicker sheets form the bottom and the cover of the packet. Ours: we pound lump charcoal in a mortar.

이 단계의 재료:

덩어리 숯(활엽수)덩어리 숯(활엽수)1 pulverized

필요한 도구:

돌 막자사발과 막자돌 막자사발과 막자
반사로반사로
대장간 집게대장간 집게
4

Hammer the packet

Hammer the packet to thin the sheets further, under a hammer whose head weighs 1,000 to 1,100 kg (2,200 to 2,400 lb). Ours: a trip hammer; the source does not say how the hammer is driven.

필요한 도구:

캠식 단조 해머캠식 단조 해머
대장간 집게대장간 집게
5

Polish under the second hammer

When the sheets are almost cold, bring them under a second hammer of the same weight with a large face, rounded at the edges, to give them polish and lustre. Do not put them back in the heating furnace.

필요한 도구:

캠식 단조 해머캠식 단조 해머
대장간 집게대장간 집게
6

Clip and sort

Let the sheets cool completely, then clip them and sort them into three classes by the perfection of their polish. A first-class sheet is like a mirror, without a spot on its surface.

필요한 도구:

판금 전단기판금 전단기

재료

2

필요 도구

6

이 블루프린트로 만드는 것

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...