Cemented Carbide

Tungsten carbide is nearly as hard as diamond and, on its own, useless: a pressed block of it shatters. The invention is not the carbide. It is the idea of cementing hard carbide grains in a small amount of tough metal, so the composite keeps most of the hardness and borrows the metal's resistance to cracking.

German patent DRP 420,689, filed 1923 by Osram Studiengesellschaft, for a method by Karl Schröter: hard materials made by pressing and sintering tungsten monocarbide with 10-20 weight-per-cent of an iron-group metal — iron, nickel or cobalt — with the binder briefly liquid so the mass densifies into a solid body. Krupp bought the patent in 1926 and marketed the product worldwide from 1927 as WIDIA, from wie Diamant, “like diamond”.

Osram's interest was not machining at all. They needed hard dies for drawing tungsten lamp filaments, and diamond dies were scarce and expensive. The cutting-tool industry was a side-effect.

초급
45 minutes

안내

1

Write the composite idea down

One line: hard grains carry the cutting, a tough binder carries the load. Neither component alone would work.

필요한 도구:

Notebook and PencilNotebook and Pencil
2

Weigh the carbide blank

Weigh the tungsten carbide round blank on the 0.01 g scale. Record the mass.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Tungsten Carbide Round Blank 1/2"Tungsten Carbide Round Blank 1/2"
Digital Scale (0.01g)Digital Scale (0.01g)
3

Measure its volume by displacement

Fill the graduated cylinder to 50 ml, lower the blank in, and read the new level. The difference is its volume in millilitres.

필요한 도구:

Graduated Cylinder (100 ml)Graduated Cylinder (100 ml)
Tungsten Carbide Round Blank 1/2"Tungsten Carbide Round Blank 1/2"
4

Calculate the density

Density = mass ÷ volume. Expect roughly 14-15 g/cm³ for a cobalt-bonded carbide.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
5

Do the same for steel

Weigh and displace a piece of the mild steel bar. Steel comes out near 7.85 g/cm³.

이 단계의 재료:

Mild Steel Square BarMild Steel Square Bar1

필요한 도구:

Digital Scale (0.01g)Digital Scale (0.01g)
Graduated Cylinder (100 ml)Graduated Cylinder (100 ml)
6

Compare the two densities

Carbide is roughly twice as dense as steel. Tungsten's atomic mass is doing that, and it is your evidence that the blank really is what it claims to be.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
7

Scratch-test steel with carbide

Drag a corner of the carbide blank across the mild steel bar with light pressure. It marks the steel easily.

이 단계의 재료:

Mild Steel Square BarMild Steel Square Bar1

필요한 도구:

Tungsten Carbide Round Blank 1/2"Tungsten Carbide Round Blank 1/2"
8

Try the reverse

Now try to scratch the carbide with an HSS cutter edge. It will not mark. Hardness is one-way, and that asymmetry is the whole ranking.

필요한 도구:

End Mill Set HSSEnd Mill Set HSS
Tungsten Carbide Round Blank 1/2"Tungsten Carbide Round Blank 1/2"
Magnifying GlassMagnifying Glass
9

Build a hardness order

Test steel, HSS, carbide and glass against each other in pairs and write them in order. You have reconstructed the logic of the Mohs scale from your own bench.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
10

Look at a carbide insert's edge

Inspect an indexable insert under the loupe. Note the blunter included angle compared with HSS — hardness bought with brittleness must be supported by geometry.

필요한 도구:

Indexable Carbide Insert Set (CCMT/TCMT)Indexable Carbide Insert Set (CCMT/TCMT)
Magnifying GlassMagnifying Glass
11

Find the indexing corners

Count the usable corners on one insert. When one dulls it is rotated, not resharpened — carbide is too hard to grind on an ordinary wheel.

필요한 도구:

Indexable Carbide Insert Set (CCMT/TCMT)Indexable Carbide Insert Set (CCMT/TCMT)
Notebook and PencilNotebook and Pencil
12

Test brittleness safely

Rest the blank on the wooden board and press its edge firmly against the steel bar. Note how unforgiving it feels — carbide chips where steel would deform. Do not strike it.

이 단계의 재료:

Flat Wooden BoardFlat Wooden Board1
Mild Steel Square BarMild Steel Square Bar1

필요한 도구:

Tungsten Carbide Round Blank 1/2"Tungsten Carbide Round Blank 1/2"
13

Write the selection rule

Interrupted cuts and flexible setups favour HSS; continuous cuts, hard material and high speed favour carbide. Write the rule in your own words.

이 단계의 재료:

Graph PaperGraph Paper1

필요한 도구:

Notebook and PencilNotebook and Pencil
14

History & Context

German patent DRP 420,689, Osram Studiengesellschaft, filed 30 March 1923 and published 30 October 1925; method by Karl Schröter. Two things are claimed: a composition — tungsten monocarbide with 10-20 wt% of an iron-group metal — and a manufacturing route, pressing and sintering with a liquid phase present. Krupp acquired the patent in 1926 and launched WIDIA (wie Diamant) in 1927.

Why a lamp company invented a cutting tool. Osram drew tungsten wire for filaments through diamond dies, which were costly and wore out. A synthetic die material was the goal; machining was an application nobody had asked for. The pattern — a material developed for one industry that reshapes another — recurs constantly in materials history.

Cobalt won. The patent lists iron, nickel or cobalt as binder. Cobalt proved best because it wets tungsten carbide grains almost perfectly during liquid-phase sintering, giving a dense body with no voids. Modern grades are still overwhelmingly WC-Co, tuned by grain size and cobalt percentage: more cobalt is tougher and less hard, less cobalt is harder and more brittle.

Why this blueprint does not sinter anything. The process needs powders at 1,400 °C, and fine cobalt powder is a genuine inhalation hazard. Solid sintered carbide — the blank and inserts used here — is inert and safe to handle. The measurements in steps 2-9 establish everything the patent claims about the material without ever making it: density proves the tungsten content, and the scratch order proves the hardness ranking.

What it displaced. High-speed steel (Taylor and White, US 668,270, 1901) gave a tool that survived at 600 °C. Carbide survives past 1,000 °C and cuts several times faster again. It did not replace HSS — drills, taps and end mills for general shop work are still largely HSS, because it can be resharpened and it tolerates flex.

재료

3

필요 도구

7

관련 블루프린트

이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...