Risers: Metal Shrinks When It Freezes, and the Hole Goes Somewhere
Almost every metal occupies less space solid than liquid. Bronze loses about 5% of its volume on freezing, steel about 3%, aluminium about 6% — and that volume has to come from somewhere.
If there is no reservoir feeding the casting, it comes out of the casting itself: a cavity, usually in the last place to freeze, usually inside a thick section where it cannot be seen until the part is machined or breaks.
A RISER is that reservoir. It is a lump of extra metal, connected to the casting, designed to stay liquid LONGER than the part it feeds — so when the casting contracts, the hole forms in the riser and the riser is cut off and remelted.
Дээд шат
3 hours
Зааварчилгаа
1
1
The riser must freeze last, which means it must be chunkier
The riser must freeze last, which means it must be chunkier
Jupyter дэвтэр ачаалж байна…
Энэ алхмын материал:
Хүрлийн гулдмай1 ширхэг
Цутгамалын элс1 кгШаардлагатай багаж:
Ширээний компьютер
Дижитал штангенциркуль 6 инч
Цутгамлын хайрцаг (дээд ба доод)2
2
Feed from the top, and keep the path open
Feed from the top, and keep the path open
Gravity does the feeding, so a riser feeds downward and sideways over a limited distance — roughly four times the section thickness along a plate, and less in alloys that freeze over a wide temperature range.
The connection between riser and casting — the riser NECK — must stay liquid until the casting has finished shrinking. A long thin neck freezes first and cuts the riser off from the part it was supposed to feed.
So the neck is short and generous, and the riser sits directly on or beside the heavy section. A riser placed at the end of a thin plate in the hope of feeding a boss at the other end feeds nothing at all.
Энэ алхмын материал:
Цутгамалын элс1 кг
Хүрлийн гулдмай1 ширхэгШаардлагатай багаж:
Цутгамлын хайрцаг (дээд ба доод)
Дижитал штангенциркуль 6 инч3
3
Open risers, blind risers, and atmospheric pressure
Open risers, blind risers, and atmospheric pressure
An OPEN riser reaches the top of the mould, so air can push down on the metal as it feeds. It also lets you see when the mould is full and top it up at the end of the pour, which is genuinely useful.
A BLIND riser is enclosed in the sand. It stays hotter because it has no exposed surface, but as the metal drains out it needs air to replace it — otherwise a vacuum forms and stops the feeding.
That is what a WHISTLER or a permeable core in the riser top is for: a small passage that lets atmospheric pressure into the riser cavity. It is a small detail that makes the difference between a blind riser working and doing nothing at all.
Энэ алхмын материал:
Цутгамалын элс1 кгШаардлагатай багаж:
Цутгамлын хайрцаг (дээд ба доод)
Шугам
Томруулагч луп4
4
Budget the metal, including everything you cut off
Budget the metal, including everything you cut off
The gating and risers can easily weigh as much as the casting. That metal is not wasted — it is cut off and remelted — but it must be MELTED, and running out mid-pour ruins the casting and the mould together.
Weigh the pattern, multiply by the ratio of alloy density to pattern-material density, and add the gating and riser volumes. Then add a margin, because a crucible is never poured completely empty.
Write the actual numbers down after the pour: what went in, what came out as casting, what came off as gating. After a few pours those figures let you predict a melt accurately, which is the difference between a foundry that works and one that improvises.
Энэ алхмын материал:
Хүрлийн гулдмай1 ширхэг
Хөнгөн цагааны гулдмай 99,7 % цэвэр, 450 г1 ширхэгШаардлагатай багаж:
Нарийн жин
ТигельМатериал
3- 1 ширхэгТүр орлуулагч
- 1 кгТүр орлуулагч
- Түр орлуулагч
Холбоотой загварууд
Эдгээр загварууд мэдлэг хуваалцдаг — арга техник, материал эсвэл зарчим

Gating: Getting the Metal In Without Wrecking the Mould
Forge зохиосон
Металл боловсруулалт
24
0
0
0
0
0

Casting Iron in a Cupola Furnace — Re-Melting Pig Iron into Finished Castings
Piett зохиосон
Металл боловсруулалт
44
0
0
0
0
0

What Heat Costs: Scale, Grain Growth and Burnt Steel
Forge зохиосон
Металл боловсруулалт
20
0
0
0
0
0
CC0 Нийтийн домэйн
Энэ загвар CC0 дор гаргагдсан. Та зөвшөөрөл авахгүйгээр хуулах, өөрчлөх, түгээх, ашиглах боломжтой.
Загвараар дамжуулан бүтээгдэхүүн худалдаж авч Бүтээгчийг дэмжээрэй Бүтээгчийн шимтгэл Борлуулагчаар тогтоосон, эсвэл энэ загварын шинэ хувилбар үүсгэж орлогоо хуваахын тулд өөрийн загварт холбоос болгон оруулна уу.