Adhesion: Four Tests, and Three of Them Destroy the Part
A plated part that looks perfect and a plated part that will peel next month are indistinguishable by eye. Adhesion has to be tested, and every worthwhile test destroys the piece it is performed on.
So the standard practice is to plate a **test coupon** alongside the real work, from the same batch, through the same baths, and to destroy that instead. A coupon costs a scrap of steel and answers the only question that matters.
The tests are simple, they need no equipment, and the failure modes each point at a different mistake earlier in the process.
Intermedio
2 hours
Instrucciones
1
1
The bend test and the burnish test
The bend test and the burnish test
**The bend test.** Bend the coupon through 180 degrees over a mandrel of a few times its thickness, then examine the outside of the bend under magnification.
A well-adhered coating **cracks with the substrate** — it may craze, but the pieces stay attached, because the coating and the metal are failing together.
A poorly adhered coating **lifts, flakes or peels away from the bend**, often in a sheet. That is a clean separation at the interface, and it means the surface was not clean.
**The burnish test.** Rub a small area briskly with a smooth hard tool — the back of a knife, a burnisher — for fifteen seconds. A well-adhered coating polishes. A poorly adhered one blisters, because the friction works it loose from underneath.
**The file test.** File across the edge of the coupon at 45 degrees, from the substrate towards the coating. A good coating is cut through cleanly; a bad one lifts ahead of the file.
**Look at the WAY it failed.** A coating that lifts in large sheets with a shiny back was on a greasy surface. One that lifts in small flakes with a dull grey back was on an oxidised one. The fracture surface names the cause.
Materiales para este paso:
Placa de acero dulce2 piezas
Chapa de níquel1 piezaHerramientas necesarias:
Lupa de relojero2
2
Thermal shock, which finds what the others miss
Thermal shock, which finds what the others miss
**Heat the part and quench it.** The coating and the substrate expand by different amounts, so a sudden temperature change puts a large shear stress directly on the interface — which is exactly what an adhesion test wants to do.
Typical: 150 to 300 C for an hour, depending on the substrate, then straight into cold water. Blistering or peeling afterwards is a fail.
**It is the most searching of the tests**, because it stresses the whole area at once rather than one line, and it finds marginal adhesion that a bend test passes.
**It doubles as the hydrogen bake.** Heating plated high-strength steel to 190 to 220 C for several hours drives dissolved hydrogen out before it can cause delayed brittle fracture, and it must be done within hours of plating. A part that both bakes and survives the quench has answered two questions.
**Do not thermal-shock a part that has been hardened**, unless the temperature is safely below its tempering temperature. The test would ruin the part in a different way.
**Record which test was used** alongside the result. "Passed adhesion" means nothing without it, in the same way that a purity figure means nothing without its method.
Materiales para este paso:
Placa de acero dulce2 piezasHerramientas necesarias:
Termómetro de laboratorio
Vaso de precipitados de borosilicato
Guantes resistentes a productos químicos3
3
Why adhesion fails, in order of likelihood
Why adhesion fails, in order of likelihood
**Contamination.** Oil, grease, a fingerprint, polishing compound, or drag-in from a previous bath. This is the great majority of failures, and the water-break test would have caught it.
**Oxide.** The part was pickled, then stood in air, then plated. A clean steel surface re-oxidises visibly in minutes and invisibly in seconds.
**Passivity.** Some metals — stainless steel, aluminium, titanium, chromium — carry an oxide film that re-forms faster than it can be removed. They need a specific activation step: a **Wood's nickel strike** for stainless, a zincate for aluminium. Plating them directly always fails, however clean they are.
**Interrupted current.** If the current stops mid-plate and then restarts, the surface passivates in the gap and the second layer does not bond to the first. A bath that has lost power is stripped and restarted, not resumed.
**Internal stress.** A highly stressed deposit — bright nickel with too much brightener, or chromium, which is always in tension — pulls itself off a marginal bond. It can peel weeks later with nothing else having changed.
**Dissimilar expansion.** A thick hard coating on a substrate with a very different expansion coefficient, in service across a temperature range.
The first two account for most of it, and both are preparation.
Materiales para este paso:
Placa de acero dulce1 pieza
Chapa de níquel1 piezaHerramientas necesarias:
Lupa de relojero4
4
Stripping and starting again
Stripping and starting again
A failed coating has to come off completely before another can go on, and a partially stripped part plates worse than a bare one.
**Chemical stripping** is the usual route and it is specific to the pair of metals. The requirement is a solution that dissolves the coating and does not attack the substrate — which is exactly the opposite of the plating chemistry, and is why a strip for nickel-on-steel is not a strip for nickel-on-brass.
**Reverse-current stripping** makes the part the anode and dissolves the coating off electrochemically. Controllable, and it stops when the coating is gone if the solution is chosen so the substrate passivates.
**Mechanical stripping** — blasting, grinding — always removes some substrate and changes the dimensions. It is the last resort on a precision part and the first choice on a rough one.
**Then start from the beginning.** A stripped part goes back through mechanical preparation, degreasing and pickling, not straight into the plating tank. The stripping solution is itself contamination.
**Consider whether it is worth it.** Stripping and replating a small part often costs more than the part. The decision is easier with a test coupon, because the failure is discovered on the coupon rather than after the part is assembled into something.
Materiales para este paso:
Ácido clorhídrico diluido al 10 %1 pieza
Placa de acero dulce1 piezaHerramientas necesarias:
Vaso de precipitados de borosilicato
Fuente de alimentación de banco ajustable
Guantes resistentes a productos químicos
Gafas de protección químicaMateriales
3- 2 piezasMarcador de posición
- 1 piezaMarcador de posición
- Marcador de posición
Herramientas requeridas
6- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.