Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate
Forge

Dicipta oleh

Forge

18. Oktober 2026NO
4
0
0
0
0

Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate

Bearing balls are headed from thick wire of 52100 steel. Here 52100 bar is forged to rod and drawn through a drawplate. At 1 % carbon it is much harder than mild steel, so it is annealed soft before drawing and again after every two holes, using the 52100 anneal Verhoeven recommends. The picture: our drawing, bar to coil.
Lanjutan
2 days

Arahan

1

Forge to rod

Heat the bar to a cherry-red heat and no hotter, and draw it out round on the anvil to a rod a little thicker than the drawplate's largest hole.

Bahan untuk langkah ini:

Batang keluli galas (52100)Batang keluli galas (52100)1 kg
ArangArang1 as required

Alatan diperlukan:

Relau tukang besiRelau tukang besi
AndasAndas
Tukul kepala baji lintangTukul kepala baji lintang
Penyepit tukang besiPenyepit tukang besi
Sarung tangan kimpalanSarung tangan kimpalan
Cermin mata keselamatanCermin mata keselamatan
2

Anneal

In the oven, hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Alatan diperlukan:

Ketuhar rawatan habaKetuhar rawatan haba
Termogandingan dengan paparanTermogandingan dengan paparan
Penyepit tukang besiPenyepit tukang besi
Sarung tangan kimpalanSarung tangan kimpalan
3

Clean and taper

Brush off all the scale, then file a long taper on the first 3 cm so it passes the first hole.

Alatan diperlukan:

Set berus dawaiSet berus dawai
Set KikirSet Kikir
Ragum BangkuRagum Bangku
4

Wax and draw

Clamp the drawplate in the vise. Wax the rod, push the taper through the first hole it does not slip through, and pull straight out with the draw tongs in one steady pull.

Bahan untuk langkah ini:

Lilin LebahLilin Lebah20 g

Alatan diperlukan:

Plat tarik keluliPlat tarik keluli
Playar tarikPlayar tarik
Ragum BangkuRagum Bangku
Sarung Tangan Kerja KulitSarung Tangan Kerja Kulit
5

Anneal every two holes

Draw through each next hole without skipping. After every two holes, coil the wire and anneal it again: hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Bahan untuk langkah ini:

Lilin LebahLilin Lebah1 keping

Alatan diperlukan:

Plat tarik keluliPlat tarik keluli
Playar tarikPlayar tarik
Ketuhar rawatan habaKetuhar rawatan haba
Termogandingan dengan paparanTermogandingan dengan paparan
6

Finish soft

Stop at the diameter your balls need, checked with the caliper, and give the coil a last anneal so it is soft for heading.

Alatan diperlukan:

Angkup Digital 6 InciAngkup Digital 6 Inci
Ketuhar rawatan habaKetuhar rawatan haba
Termogandingan dengan paparanTermogandingan dengan paparan
7

Troubleshooting

Bearing steel wire troubleshooting.

Flow

Loading...

Bahan

3

Alatan Diperlukan

15

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...