Carbon Resistance Ring: Laminated Paper Gelled with 15% Tung Oil, Graphite-Shellac Track
Mallory's quiet volume-control ring (US 2,144,925, 1939). Hard bases were noisy and soft paper ones changed with damp. Their answer: paper rings soaked in 15 % raw tung oil and baked, so the oil gels inside the paper. It shuts out moisture but stays soft and springy, and the wiper runs on it quietly. A graphite paint makes the track, silver paint the ends.
The picture: the patent's drawing (Fig. 3).
Pertengahan
1 day
Arahan
1
1
Punch rings from three-ply paper
Punch rings from three-ply paper
The base is three papers stuck into one sheet: litho paper at the back, newsprint in the middle, manila on the face that takes the track. Punch rings from it. Ours: a punch press with a ring die.
Bahan untuk langkah ini:
Kertas Berlamina Tiga Lapis1 kepingAlatan diperlukan:
Mesin penekan tebuk
Acuan Tebuk Cincin
Sarung tangan getah2
2
Soak 1 hour in 15 % tung oil in naphtha
Soak 1 hour in 15 % tung oil in naphtha
Soak the rings for about one hour in about 15 % raw tung oil in naphtha. Use raw oil, not heat-bodied or treated oil, so it can still gel.
Bahan untuk langkah ini:
Minyak tung15 partsAlatan diperlukan:
Nafta
Bikar Kaca
Neraca dua piring
Pengacau
Alat pernafasan muka penuh
Sarung tangan getah3
3
Air-dry, then bake at 210–250 °C
Air-dry, then bake at 210–250 °C
Dry the rings in air for two hours or more, then bake 15 to 30 minutes at 210 to 250 °C. The oil gels in the paper's pores; the paper stays pliable.
Alatan diperlukan:
Ketuhar pengeringan
Termometer Ketuhar
Sarung Tangan Tahan Haba4
4
Spray the graphite track
Spray the graphite track
Spray on the resistance paint, for example graphite in a shellac binder. The patent gives no proportions. The track can be tapered in thickness, width or mix to shape the resistance curve.
Bahan untuk langkah ini:
Serbuk Grafit1 as required
Selak1 as requiredAlatan diperlukan:
Pistol Semburan
Pemampat udara
Alat pernafasan muka penuh
Sarung tangan getah5
5
Paint silver ends, bake at 220 °C
Paint silver ends, bake at 220 °C
Spray or paint the two end terminals with silver particles in shellac. Dry, then bake at about 220 °C to cure and harden the track. The slight warp from soaking flattens out again.
Bahan untuk langkah ini:
Cat perak konduktif1 as requiredAlatan diperlukan:
Pistol Semburan
Ketuhar pengeringan
Termometer Ketuhar
Sarung Tangan Tahan HabaBahan
5- 1 kepingPemegang Tempat
- 15 partsPemegang Tempat
- 1 as requiredPemegang Tempat
- 1 as requiredPemegang Tempat
- 1 as requiredPemegang Tempat
Alatan Diperlukan
13- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- Pemegang Tempat
- 1 vendor sell this, none ship to you yetPemegang Tempat
Blueprint ini membuat
Blueprint berkaitan
Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip
CC0 Domain Awam
Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.
Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.