Claw Hammer: Drop-Forged Head, Turned Wooden Handle
Forge

Dicipta oleh

Forge

11. Oktober 2026NO
33
0
0
0
0

Claw Hammer: Drop-Forged Head, Turned Wooden Handle

A claw hammer's head is high-carbon steel, hot forged between dies and then hardened only where it takes the blows: the face, the poll and the claws. The handle is straight-grained ash or hickory, woods with good strength, durability and enough give to absorb the shock of repeated blows. It is turned on a lathe that copies a cam, pushed up through the head's eye and wedged: one thin wooden wedge driven diagonally into a slot, then two steel wedges driven through it crossways.
Lanjutan
Factory process

Arahan

1

Heat the bar

Heat a length of steel bar to about 1,200–1,300 °C (2,200–2,350 °F) with open flame torches or by passing it through an induction coil.

Bahan untuk langkah ini:

Bar keluli alat segi empat samaBar keluli alat segi empat sama1 as required

Alatan diperlukan:

Pemanas aruhanPemanas aruhan
2

Forge the head

Put the hot bar or a cut blank between the dies. The ram forces them together and squeezes the steel into the die cavities; repeat in several dies to form the head step by step.

Alatan diperlukan:

Tukul jatuh dengan dai tempaTukul jatuh dengan dai tempa
3

Trim the flash

Cut off the flash, the steel squeezed out between the dies, with trimming dies. Cool the head and grind off rough spots.

Alatan diperlukan:

Dai penanggal siripDai penanggal sirip
Pengisar mejaPengisar meja
4

Harden the face, poll and claws

Heat those areas with a flame or an induction coil and cool them quickly, so the steel near the surface becomes much harder than the rest of the head.

Alatan diperlukan:

Pemanas aruhanPemanas aruhan
5

Clean and polish

Shot blast the head (a stream of air carrying small steel particles), paint it if wanted, then polish the face, poll, claws and cheeks. Smooth the V-slot of the claws with an abrasive disc.

Alatan diperlukan:

Kabinet letupan syotKabinet letupan syot
Roda penggilapRoda penggilap
6

Turn the handle

Cut ash or hickory to length and hold it at both ends in the lathe. As it spins, the cutting tool follows a cam with the handle's shape. Cut a slot diagonally across the top and sand the handle smooth.

Bahan untuk langkah ini:

Batang Kayu Keras untuk HuluBatang Kayu Keras untuk Hulu1 keping

Alatan diperlukan:

Mesin larik pemegang berpandu sesondolMesin larik pemegang berpandu sesondol
Kertas PasirKertas Pasir
7

Hang the head

Push the handle up through the eye of the head. Tap the wooden wedge into the diagonal slot to spread the handle against the head, then drive two small steel wedges through it crossways.

Bahan untuk langkah ini:

Pasak kayu kerasPasak kayu keras1 keping
Baji silang keluliBaji silang keluli2 keping

Bahan

4

Alatan Diperlukan

8

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...