Crucible Furnace: the Brass Founder's Sunk Coke Air Furnace (Larkin, 1907)
Forge

Dicipta oleh

Forge

3. November 2026NO
7
0
0
1
0

Crucible Furnace: the Brass Founder's Sunk Coke Air Furnace (Larkin, 1907)

The brass founder's crucible furnace: a firebrick-lined pit sunk below the floor, fired with hard coke on an iron grating over the ash-pit, closed by a dome-shaped iron cover and drawn by a flue with a damper. The crucible sits on a firebrick in the middle of the fire, lidded, with coke banked round it, until the metal is melted. Result: a coke-fired crucible furnace for melting brass and bronze. Source: J. Larkin, The Practical Brass and Iron Founder's Guide (1907), pp. 96-99. Unknown: all sizes. Picture drawn by Youblob.
Pertengahan
Unknown

Arahan

1

Build the pit

Sink the furnace below the floor. Line the inside with firebricks set in fireclay; use pure clay (white, opaque, oily to the touch), since iron oxide, magnesia, lime or black lead in brick or clay shortens the furnace's life. Close the ash-pit at the bottom with a hinged iron grating. Not given: sizes.

Bahan untuk langkah ini:

Bata Tahan ApiBata Tahan Api1 lining
Tanah Liat Tahan ApiTanah Liat Tahan Api1 jointing
Logam tidak diketahuiLogam tidak diketahui1 hinged grating

Alatan diperlukan:

Dimensi tidak diketahuiDimensi tidak diketahui
2

Fit the cover and flue

Make a dome-shaped cover for the furnace top of cast or wrought iron. Lead a flue from the furnace with a damper in it. Not given: the flue size or height.

Bahan untuk langkah ini:

Logam tidak diketahuiLogam tidak diketahui1 dome cover, damper
Paip serombongPaip serombong1 flue

Alatan diperlukan:

Dimensi tidak diketahuiDimensi tidak diketahui
3

Fire it and melt

Burn hard coke broken to lumps the size of a fist. Heat the crucible bottom upwards in the fire, lift it out with the tongs, turn it upright and bed it on a slab of fireclay or a firebrick, put on its lid and bank the fire round it. Put the metal in, close the cover and open the damper for draught until the metal is melted. Black-lead crucibles last longer; clay ones must first be hardened by slowly raising their temperature.

Alatan diperlukan:

Kok metalurgiKok metalurgi
Mangkuk pijar grafit-tanah liatMangkuk pijar grafit-tanah liat
Penyepit Mangkuk PijarPenyepit Mangkuk Pijar

Bahan

4

Alatan Diperlukan

4

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...