Steel Files: Forged, Cut and Hardened
Forge

Dicipta oleh

Forge

11. Oktober 2026NO
29
0
0
0
0

Steel Files: Forged, Cut and Hardened

A file is a bar of high-carbon steel, about 1.0–1.25 % carbon, covered in rows of tiny chisel cuts. The blank is forged with a tang, annealed soft, ground flat, and the teeth are raised one by one with a chisel and hammer: each blow cuts a groove and lifts its edge into a tooth. A single-cut file has one row of parallel cuts, at 65–85° to the length; a double-cut file has a second row crossing the first, for general work the first at 40–45° and the second at 70–80°. The file is then hardened as hard as it will go by quenching it in cold brine, and is never tempered; only the tang is softened so it will not snap. Factories do the same steps by machine.
Lanjutan
2 days (annealing overnight)

Arahan

1

Forge the blank

At a yellow heat, draw the high-carbon steel to the file's section and forge a narrow, pointed tang at one end.

Bahan untuk langkah ini:

Bilet keluli karbon tinggiBilet keluli karbon tinggi0.5 kg

Alatan diperlukan:

Relau tukang besiRelau tukang besi
AndasAndas
Tukul TempaTukul Tempa
Penyepit Tukang BesiPenyepit Tukang Besi
2

Anneal

Heat the blank no hotter than a blood-red and let it cool very slowly, shut away from the air; factories leave blanks in closed boxes in the furnace for 24–36 hours. Cooled in open air it would harden again.

Alatan diperlukan:

Relau tukang besiRelau tukang besi
3

Straighten and grind

Straighten the blank, grind off the scale and make the faces flat and even, or the teeth will not be uniform.

Alatan diperlukan:

Batu canai rodaBatu canai roda
4

Cut the teeth

Hold the chisel at an angle and strike it, then move it a small, regular distance and strike again; each blow raises one tooth. For a double cut, cut the first row (overcut), then a second row crossing it (upcut). To cut the other face, turn the file over on a pewter plate so the finished teeth are not crushed.

Alatan diperlukan:

Pahat pembuat gigi kikirPahat pembuat gigi kikir
Tukul TempaTukul Tempa
AndasAndas
Plat piuterPlat piuter
5

Harden

Heat the file evenly to its hardening heat and plunge it into a bath of cold brine, which cools faster than water and leaves it harder. Do not temper it.

Bahan untuk langkah ini:

GaramGaram1 kg

Alatan diperlukan:

Relau tukang besiRelau tukang besi
BaldiBaldi
Penyepit Tukang BesiPenyepit Tukang Besi
6

Soften the tang

Reheat the tang alone so it is no longer glass-hard: a fully hard tang snaps when the handle is driven on. Clean and oil the file.

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Penyepit Tukang BesiPenyepit Tukang Besi

Bahan

2

Alatan Diperlukan

8

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...