Rasps: Teeth Raised One at a Time with a Pointed Punch
Forge

Dicipta oleh

Forge

11. Oktober 2026NO
32
0
0
0
0

Rasps: Teeth Raised One at a Time with a Pointed Punch

A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
Lanjutan
2 days (annealing overnight)

Arahan

1

Forge the blank

Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.

Bahan untuk langkah ini:

Bilet keluli karbon tinggiBilet keluli karbon tinggi0.5 kg

Alatan diperlukan:

Relau tukang besiRelau tukang besi
AndasAndas
Tukul TempaTukul Tempa
Penyepit Tukang BesiPenyepit Tukang Besi
2

Anneal and grind

Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.

Alatan diperlukan:

Relau tukang besiRelau tukang besi
Batu canai rodaBatu canai roda
3

Punch the teeth

Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.

Alatan diperlukan:

Penebuk kikir kasarPenebuk kikir kasar
Tukul TempaTukul Tempa
AndasAndas
Plat piuterPlat piuter
4

Harden

Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.

Bahan untuk langkah ini:

GaramGaram1 kg
Kok metalurgiKok metalurgi1 as required

Alatan diperlukan:

Relau tukang besiRelau tukang besi
BaldiBaldi
Penyepit Tukang BesiPenyepit Tukang Besi
5

Temper the tang and clean

Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.

Alatan diperlukan:

Takungan plumbum leburTakungan plumbum lebur
Penyepit Tukang BesiPenyepit Tukang Besi

Bahan

3

Alatan Diperlukan

9

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...