PET (polyethylene terephthalate) was invented by Whinfield and Dickson, whose patent (US 2,465,319, 1949) gives this first example: boil terephthalic acid in ethylene glycol until it dissolves, wash and dry the glycol ester, then heat it at 280 °C under nitrogen until it is a viscous polymer that melts at 254–255 °C and can be drawn into fibre. The melt is extruded and cut into chips (pellets) for moulding and spinning. The picture: our diagram.
Lanjutan
About 4 days

Arahan

1

Boil the acid in glycol

Reflux 50 g terephthalic acid with 89 g ethylene glycol for about 72 hours, until it has all dissolved. This makes glycol terephthalate.

Bahan untuk langkah ini:

Asid TereftalikAsid Tereftalik50 g
Etilena glikolEtilena glikol89 g

Alatan diperlukan:

Neraca dua piringNeraca dua piring
Kelalang dasar bulatKelalang dasar bulat
Gegelung kondenserGegelung kondenser
Plat PemanasPlat Pemanas
2

Wash and dry the ester

Wash the glycol terephthalate with water and dry it under vacuum.

Alatan diperlukan:

Air SulingAir Suling
Corong Kaca BertangkaiCorong Kaca Bertangkai
Kertas TurasKertas Turas
Pam vakumPam vakum
3

Heat at 280 °C under nitrogen

Melt it and heat at 280 °C for 8½ hours in a slow stream of nitrogen: no air may reach it. It grows thick as it polymerises.

Alatan diperlukan:

Kelalang dasar bulatKelalang dasar bulat
Plat PemanasPlat Pemanas
Termogandingan dengan paparanTermogandingan dengan paparan
Silinder Gas NitrogenSilinder Gas Nitrogen
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
Gogal Percikan KimiaGogal Percikan Kimia
4

Test for cold-drawing

Pull a thread from the melt with a rod and let it cool. It is ready when the cold thread can be stretched to several times its length. The finished polymer melts at 254–255 °C.

Alatan diperlukan:

Rod Pengacau KacaRod Pengacau Kaca
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba
5

Extrude and cut into chips

Extrude the molten polymer, let it cool, and cut it into chips (pellets).

Alatan diperlukan:

Penyemperit plastikPenyemperit plastik
PemeletPemelet
Sarung Tangan Tahan HabaSarung Tangan Tahan Haba

Bahan

2

Alatan Diperlukan

15

Blueprint berkaitan

Blueprint ini berkongsi pengetahuan — teknik, bahan atau prinsip

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...