Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)

An air furnace melts iron apart from the fuel: coal burns on a grate at one end, and the flame is thrown down from a low arched roof onto the iron on the bed, then leaves by a tall chimney. The iron stays cleaner than in a cupola, so founders used it for guns, rolls, heavy scrap and lumps too big for the cupola. This furnace is 30 ft 6 in long and 7 ft wide outside, 5 ft wide inside, cased in bolted wrought-iron plates. Source: S. Bolland, The Iron Founder Supplement (1893), pp. 55-67. Unknown: brick sizes, plate thickness. Picture: Fig. 14 of the book.
Pakar
Unknown

Arahan

1

Lay the foundation

Build the foundation solid of common material up to the firebrick, shaped so the firebrick bed slopes down from the chimney end to the reservoir. Keep the bricks from B to C 6 in below the finished bottom, to leave room for the sand bed.

Bahan untuk langkah ini:

BataBata1 foundation

Alatan diperlukan:

Sudip tukangSudip tukang
Dimensi tidak diketahuiDimensi tidak diketahui
2

Build the fireplace, bridge and roof

Build the fireplace the full width of the furnace (5 ft inside, grate 5 ft long). Set the bridge wall at least 2 ft 3 in from the face of the grate bars. Build bridge, sides, roof and fireplace of the most refractory firebrick. Arch the roof the whole length, low, so it throws the flame down onto the bed; fill above the arches with common material. Leave the side charging hole (5 x 4 ft), the top hole (furnace width x 6 ft), the puddling hole over the reservoir, a sight hole and the tap hole.

Bahan untuk langkah ini:

Batu tanah apiBatu tanah api1 lining, bridge, roof
Mortar tanah liat tahan apiMortar tanah liat tahan api1 setting
BataBata1 filling above the arch
Logam tidak diketahuiLogam tidak diketahui1 grate bars

Alatan diperlukan:

Sudip tukangSudip tukang
3

Case it in plates and bolt it

Case the whole structure in wrought-iron plates, held at the corners with angle-irons. Run eight chief anchor bolts from side to side, clear of all working parts. Join everything with bolts, not rivets, so any plate can come off for repairs. Line the charging doors with firebrick.

Bahan untuk langkah ini:

Plat besiPlat besi1 casing, doors
Rod besi tempaRod besi tempa8 anchor bolts
Logam tidak diketahuiLogam tidak diketahui1 angle-irons, door frames
Batu tanah apiBatu tanah api1 door linings

Alatan diperlukan:

Dimensi tidak diketahuiDimensi tidak diketahui
4

Build the chimney

Build the chimney square, 30 to 40 ft high, with an inside course of firebrick (Fig. 14: 2 ft 6 in square inside). Make its area a little larger than the fireplace. Put a damper on top that can be worked from the bottom: it alone sets the draught. It can stand apart on a sole plate on four columns.

Bahan untuk langkah ini:

Batu tanah apiBatu tanah api1 inside course
BataBata1 chimney
Logam tidak diketahuiLogam tidak diketahui1 damper

Alatan diperlukan:

Sudip tukangSudip tukang
5

Make the sand bottom

Make the bottom from B round the reservoir to C with 8 parts fire-sand to 1 of clay and 1 of ground coke. Fire it well for one to two hours before the first charge; it should last ten heats. Fill the tap hole with fire-sand and a little coal dust, which will not cake when hot.

Bahan untuk langkah ini:

PasirPasir8 parts
Tanah LiatTanah Liat1 part
Kok metalurgiKok metalurgi1 part, ground

Alatan diperlukan:

Arang batu bituminusArang batu bituminus
6

Charge and melt

Fire with soft, non-caking bituminous coal and keep a full grate; clinker quickly and leave no holes for cold air. Charge all the iron at the start: first layer of pigs lengthwise and a little apart, next layers across, open so the flame passes. Set heavy pieces on firebricks so the flame plays all round them. Through the puddling hole, dip test pieces and skim the iron clean. To blend two grades, thrust green saplings into the melt. Close the damper before tapping. Look the furnace over after every heat.

Alatan diperlukan:

Arang batu bituminusArang batu bituminus
Jongkong besi mentahJongkong besi mentah
Batang Anak Pokok Kayu KerasBatang Anak Pokok Kayu Keras
Penyenduk berlubangPenyenduk berlubang

Bahan

9

Alatan Diperlukan

6

CC0 Domain Awam

Blueprint ini dikeluarkan di bawah CC0. Anda bebas menyalin, mengubah, mengedar, dan menggunakan karya ini untuk sebarang tujuan, tanpa meminta kebenaran.

Sokong Pembuat dengan membeli produk melalui Blueprint mereka di mana mereka memperoleh Komisen Pembuat ditetapkan oleh Penjual, atau cipta iterasi baru Blueprint ini dan sertakan ia sebagai sambungan dalam Blueprint anda sendiri untuk berkongsi hasil.

Perbincangan

(0)

Log masuk untuk menyertai perbincangan

Memuatkan komen...