Butyraldehyde: Butyl Alcohol Dehydrogenated over Copper Pellets at 400-680 °F (Hasche, Eastman, US 2,173,111)

Hot copper pulls two hydrogen atoms off butyl alcohol and leaves butyraldehyde. Hasche's catalyst is copper made from blown, water-quenched cuprous oxide, in dust-free pellets that can be burnt clean and reduced again when they tire. Result: butyraldehyde, distilled off from the unchanged alcohol. Source: Hasche, US 2,173,111 (Eastman Kodak, 1939), claims 6, 9 and 12. His worked run is for propyl alcohol; conversion for butanol is not given. Picture drawn by Youblob.
Ilọsíwájú
1 day

Ìlànà

1

Pack the copper catalyst

Fill a tube with dust-free copper pellets made from cuprous oxide blown from molten copper and quenched in water (2-5 mesh in claim 17).

Àwọn irinṣẹ́ tí a nílò:

Wóró ohun ìmúyára bàbàWóró ohun ìmúyára bàbà
Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
2

Preheat the butyl alcohol

Vaporise and preheat the butyl alcohol to about 500-600 °F.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

n-Butanoln-Butanol1 as required

Àwọn irinṣẹ́ tí a nílò:

Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
3

Pass it over the copper at 400-680 °F

Lead the hot vapour over the catalyst held at about 400-680 °F. It splits into butyraldehyde and hydrogen; part of the alcohol passes unchanged.

Àwọn irinṣẹ́ tí a nílò:

Wóró ohun ìmúyára bàbàWóró ohun ìmúyára bàbà
Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
Ìyípo ẹ̀rọ ìtutùÌyípo ẹ̀rọ ìtutù
4

Distil off the aldehyde

Condense the products and distil: butyraldehyde comes over first (it boils near 74 °C); distil the alcohol back in the presence of alkali and return it.

Àwọn irinṣẹ́ tí a nílò:

Ohun ìsun tí ó pínOhun ìsun tí ó pín
Sodium hydroxide ní omi ìdá 10Sodium hydroxide ní omi ìdá 10
5

Reactivate the spent copper

When the catalyst slows, flush it, oxidise it at about 600-800 °F, cool, and reduce it again with alcohol vapour at about 300-400 °F.

Àwọn irinṣẹ́ tí a nílò:

Wóró ohun ìmúyára bàbàWóró ohun ìmúyára bàbà
Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n

Àwọn ohun-èlò

1
  • 1 as required
    Àyè

Àwọn irinṣẹ́ tó nílò

5

Ìtọ́nisọ́nà yìí ń ṣe

Blueprint tó jọra

Àwọn blueprint wọ̀nyí pín ìmọ̀ — ọ̀nà, ohun-èlò tàbí ìlànà

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...