Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)
Charlie

Ṣẹ́dá nipasẹ̀

Charlie

28. Oṣù Kẹwà 2026DE
2
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)

A strontium ferrite with 0.06 mol strontium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 23. Went's rod held 2,120 gauss with a coercive force of 1,950 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 24. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Ilọsíwájú
2 days

Ìlànà

1

Weigh the carbonates and iron oxide

Weigh 8.86 g strontium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol), 95.55 g ferric oxide (0.6 mol). The patent prints 81.86 g of strontium carbonate beside 0.06 mol. 0.06 mol is 8.86 g (ours, at 147.63 g per mol), the weight used here.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Strontium carbonateStrontium carbonate8.86 g
Calcium carbonate (ẹfun funfun)Calcium carbonate (ẹfun funfun)4.004 g
Ọ́kísáìdì irin (III)Ọ́kísáìdì irin (III)95.55 g

Àwọn irinṣẹ́ tí a nílò:

Òǹwọ̀n ìdọ́gbaÒǹwọ̀n ìdọ́gba
Ẹ̀rọ Ìmí P100Ẹ̀rọ Ìmí P100
2

Mill with alcohol 4 hours, dry

As in Example 23: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ Lílọ Bọ́ọ̀lù IrinẸ̀rọ Lílọ Bọ́ọ̀lù Irin
Ethanol - ìpele ilé-ìwádìí, 95 %Ethanol - ìpele ilé-ìwádìí, 95 %
Ààrò ìgbẹ̀Ààrò ìgbẹ̀
3

Press at 1.5 t/cm²

Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Àwọn irinṣẹ́ tí a nílò:

Ẹ̀rọ ìtẹ̀ háídírọ́líìkìẸ̀rọ ìtẹ̀ háídírọ́líìkì
Mọ́ọ̀dù títẹ díìsìMọ́ọ̀dù títẹ díìsì
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Àwọn irinṣẹ́ tí a nílò:

Ààrò Ọ̀pọ́nÀàrò Ọ̀pọ́n
Ìbọ̀wọ́ Tí Ń Fara Da OoruÌbọ̀wọ́ Tí Ń Fara Da Ooru
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Àwọn irinṣẹ́ tí a nílò:

Òòfà iná-mànàmánáÒòfà iná-mànàmáná
Kọ́mpasiKọ́mpasi

Àwọn ohun-èlò

3

Àwọn irinṣẹ́ tó nílò

11

Ìtọ́nisọ́nà yìí ń ṣe

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...