Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)
Charlie

सिर्जनाकर्ता

Charlie

28. अक्टोबर 2026DE
२
०
०
०
०

Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)

Ordinary soaps stop tetrafluoroethylene from growing into long chains. A fluorine soap does not: with 2 % of ammonium dodecafluoroheptanoate in the water, the gas polymerises into tiny PTFE ribbons that stay suspended. The result is a milky dispersion, a third of it polymer, the raw material for PTFE fine powder. Source: K. L. Berry (du Pont), US 2,559,752 (1951), Example III. Making the ammonium salt from our acid, and the apparatus, are ours. Picture drawn by Youblob.
उन्नत
1 day

निर्देशनहरू

1

Make the ammonium salt

Ours: neutralise about 1.9 parts of dodecafluoroheptanoic acid with ammonia solution until just neutral to litmus, giving 2 parts of ammonium dodecafluoroheptanoate. Make it up with distilled water to 93 parts of water in all. Parts are by weight.

यस चरणका सामग्री:

डोडेकाफ्लोरोहेप्टानोइक अम्लडोडेकाफ्लोरोहेप्टानोइक अम्ल1.9 parts
अमोनियाको घोल - २५-२८ %अमोनियाको घोल - २५-२८ %1 as required to neutralise
आसुत पानीआसुत पानी93 parts

चाहिने औजार:

लिटमस कागजलिटमस कागज
सिसाको भाँडोसिसाको भाँडो
समभुज तराजुसमभुज तराजु
2

Load the pressure vessel

Put the solution in a pressure vessel with 0.05 part of potassium persulfate and 5 parts of paraffin wax melting at 56–58 °C. The wax protects the colloid while it is stirred.

चाहिने औजार:

पर्सल्फेट आरम्भकपर्सल्फेट आरम्भक
प्यारफिन मैनप्यारफिन मैन
चाप रिएक्टरचाप रिएक्टर
समभुज तराजुसमभुज तराजु
3

Heat and remove the air

Bring it to 80–85 °C, then evacuate the vessel and hold it under reduced pressure for several minutes to drive out air and dissolved oxygen.

चाहिने औजार:

चाप रिएक्टरचाप रिएक्टर
निर्वात पम्पनिर्वात पम्प
तापमापकतापमापक
4

Feed tetrafluoroethylene for 3.6 hours

Let in tetrafluoroethylene to 60 lb/sq in gauge. Agitate at 80–85 °C for 3.6 hours; each time the pressure falls to 55 lb/sq in, bring it back to 60.

यस चरणका सामग्री:

टेट्राफ्लोरोइथिलिनटेट्राफ्लोरोइथिलिन1 as required to hold 55–60 psi

चाहिने औजार:

चाप रिएक्टरचाप रिएक्टर
चापयुक्त ग्यासको सिलिन्डरचापयुक्त ग्यासको सिलिन्डर
चापमापकचापमापक
तापमापकतापमापक
5

Cool and lift off the wax

Cool it. The paraffin sets on top and lifts off. Below it is a colloidal PTFE dispersion with 34 % solids.

चाहिने औजार:

चाप रिएक्टरचाप रिएक्टर
बिर्को भएको सिसाको भाँडोबिर्को भएको सिसाको भाँडो

सामग्री

4

आवश्यक उपकरणहरू

11

CC0 सार्वजनिक डोमेन

यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।

ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।

छलफल

(0)

लग इन छलफलमा सामेल हुन

टिप्पणीहरू लोड गर्दै...