Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days
निर्देशनहरू
1
1
Weigh one part barium carbonate to six of iron oxide
Weigh one part barium carbonate to six of iron oxide
Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.
यस चरणका सामग्री:
ब्यारियम कार्बोनेट (विथराइट)39.5 ग्राम
फेरिक अक्साइड191.7 ग्रामचाहिने औजार:
समभुज तराजु
रबरका पन्जा
P100 स्वास रक्षक2
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
चाहिने औजार:
फलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टी3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
चाहिने औजार:
मफल भट्टी
बिर्कोसहितको क्रुसिबल (चिनियाँ माटो)
मुसाको चिम्टा
ताप सहने पन्जा4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
चाहिने औजार:
फलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टी
P100 स्वास रक्षक5
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
चाहिने औजार:
हाइड्रोलिक प्रेस
डिस्क थिच्ने डाइ6
6
Sinter for 4 hours
Sinter for 4 hours
Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.
चाहिने औजार:
मफल भट्टी
मुसाको चिम्टा
ताप सहने पन्जा7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
चाहिने औजार:
विद्युत् चुम्बक
दिशासूचक यन्त्रसामग्री
2- 39.5 ग्रामप्लेसहोल्डर
- 191.7 ग्रामप्लेसहोल्डर
आवश्यक उपकरणहरू
14- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
सम्बन्धित ब्लुप्रिन्ट
यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।