Barium Sulphide: Heavy Spar Roasted with Coal
Barium sulphide is the barium half of lithopone, the white pigment. Thorpe (1912): roast 100 parts of heavy spar with 20 parts of coal slack or charcoal. Caking bituminous coal soaks through the mass and reduces it completely; with charcoal, mix very thoroughly. The roasted mass still holds carbon and some unchanged spar: hot water takes out the barium sulphide. Left in air it turns to carbonate and smells of rotten eggs, so keep it closed.
The picture: our own drawing.
मध्यम
1 day
निर्देशनहरू
1
1
Grind and mix
Grind and mix
Grind 100 g of heavy spar and 20 g of bituminous coal slack and mix them very thoroughly.
यस चरणका सामग्री:
बराइट (भारी स्पार)100 ग्रामचाहिने औजार:
बिटुमिनी कोइला
खल र लोहोरो
समभुज तराजु2
2
Roast
Roast
Roast the mixture in a crucible in the furnace. The coal cakes and runs through the mass, reducing the spar.
चाहिने औजार:
गहिरो माटोको मुसा
कोइलाको भट्टी
छालाका पन्जा3
3
Cool and close it up
Cool and close it up
Let it cool and put it straight into an airtight jar. It holds spare carbon and some unchanged spar; hot water dissolves out the barium sulphide when you use it.
चाहिने औजार:
हावा नछिर्ने बिर्को भएका गाढा काँचका भाँडा
छालाका पन्जासामग्री
1- 100 ग्रामप्लेसहोल्डर
आवश्यक उपकरणहरू
7- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।