A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Gray found this paint so stable that it kept six months. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 2. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
शुरुआती
1 day

निर्देशनहरू

1

Dissolve 2 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.

यस चरणका सामग्री:

पोलिभिनाइल अल्कोहल धुलोपोलिभिनाइल अल्कोहल धुलो2 ग्राम
आसुत पानीआसुत पानी1 as required

चाहिने औजार:

समभुज तराजुसमभुज तराजु
बोरोसिलिकेट बिकरबोरोसिलिकेट बिकर
तताउने प्लेटतताउने प्लेट
बोरोसिलिकेट काँचको डण्डीबोरोसिलिकेट काँचको डण्डी
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

यस चरणका सामग्री:

सिल्भर अक्साइडसिल्भर अक्साइड50 ग्राम
बिस्मथ सबनाइट्रेटबिस्मथ सबनाइट्रेट1 as required

चाहिने औजार:

समभुज तराजुसमभुज तराजु
खल र लोहोरोखल र लोहोरो
नाइट्राइल पन्जानाइट्राइल पन्जा
3

Add 2 to 4 g alcohol against foam

Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.

यस चरणका सामग्री:

इथानोल - प्रयोगशाला श्रेणी, 95 %इथानोल - प्रयोगशाला श्रेणी, 95 %1 as required

चाहिने औजार:

बोरोसिलिकेट काँचको डण्डीबोरोसिलिकेट काँचको डण्डी
4

Store

Keep it in a closed jar. Gray found no reaction between the ingredients in six months, and the paint can stand for some hours in use without stirring.

चाहिने औजार:

हावा नछिर्ने बिर्को भएका गाढा काँचका भाँडाहावा नछिर्ने बिर्को भएका गाढा काँचका भाँडा

सामग्री

5

आवश्यक उपकरणहरू

7

सम्बन्धित ब्लुप्रिन्ट

यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त

CC0 सार्वजनिक डोमेन

यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।

ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।

छलफल

(0)

लग इन छलफलमा सामेल हुन

टिप्पणीहरू लोड गर्दै...