Methyl Methacrylate Syrup: Partly Polymerised below 80 °C with Hydrogen Peroxide
Methyl methacrylate syrup is the monomer partly polymerised until it is thick: the stock that is poured between glass plates to cast acrylic sheet. ICI's Tattersall (US 2,071,907, 1937) heats the liquid monomer with a little catalyst, never above 80 °C, until it is syrupy, then cools it. His example used benzoyl peroxide and he names hydrogen peroxide as an alternative but gives no amount. Our choice: 14 g of 3 % hydrogen peroxide per kg of monomer, as many peroxide molecules as his 0.3 % benzoyl peroxide. Methyl methacrylate is flammable: no open flame.
The picture: our diagram.
मध्यम
Half a day
निर्देशनहरू
1
1
Weigh monomer and peroxide
Weigh monomer and peroxide
Weigh liquid methyl methacrylate into a round-bottom flask and add 14 g of 3 % hydrogen peroxide per kg of monomer (our amount; the patent only says a relatively small amount).
यस चरणका सामग्री:
मिथाइल मेथाक्रिलेट1 केजी
हाइड्रोजन पेरोक्साइड (३ %)14 ग्रामचाहिने औजार:
गोलो पिँधको फ्लास्क
समभुज तराजु
रासायनिक छिटाको चस्मा
रबरका पन्जा
धुवाँ कक्ष (नली भएको)2
2
Heat, never above 80 °C
Heat, never above 80 °C
Fit a reflux condenser and warm the flask in a water bath to near but not above 80 °C. Above 80 °C the finished sheet is not flawless; lower temperatures work but take longer.
चाहिने औजार:
गोलो पिँधको फ्लास्क
रिफ्लक्स कन्डेन्सर
वाटर बाथ
तताउने प्लेट
प्रयोगशाला तापमापक
धुवाँ कक्ष (नली भएको)3
3
Stop when it is syrupy
Stop when it is syrupy
Check the thickness now and then with a glass rod. Stop when the liquid has become a syrup. The patent took its example to a molecular weight of 3000, measured by viscosity, and gives no time.
चाहिने औजार:
सिसाको चलाउने डण्डी
प्रयोगशाला तापमापक4
4
Cool to room temperature
Cool to room temperature
Cool the syrup to about room temperature (30 °C in the example) in cold water. It is then ready to pour between glass plates and cast into sheet.
चाहिने औजार:
पानीले चिसो पार्ने कुण्ड
प्रयोगशाला तापमापक
रबरका पन्जासामग्री
2- 1 केजीप्लेसहोल्डर
- 14 ग्रामप्लेसहोल्डर
आवश्यक उपकरणहरू
11- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
सम्बन्धित ब्लुप्रिन्ट
यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।