Metal Oxide Varistor: Zinc Oxide, 0.5 % Bismuth Oxide, 0.2 % Manganese Dioxide, 1350 °C (Masuyama 1972, Ex. 2)
Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with manganese dioxide: 99.3 % zinc oxide, 0.5 % bismuth oxide and 0.2 % manganese dioxide by moles, sintered at 1350 °C. The disc measured a C-value of 90 at 1 mA and a nonlinearity exponent n of 11.5.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
उन्नत
1 day
निर्देशनहरू
1
1
Weigh 99.3 : 0.5 : 0.2 and wet-mill 5 hours
Weigh 99.3 : 0.5 : 0.2 and wet-mill 5 hours
Mix zinc oxide, bismuth oxide and manganese dioxide 99.3 : 0.5 : 0.2 by moles. Ours, for 10 g: 9.699 g zinc oxide, 0.28 g bismuth oxide, 0.021 g manganese dioxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.
यस चरणका सामग्री:
जिंक अक्साइड धुलो9.699 ग्राम
बिस्मथ अक्साइड0.28 ग्राम
म्याङ्गनिज डाइअक्साइड (पाइरोलुसाइट)0.021 ग्रामचाहिने औजार:
समभुज तराजु
फलामे बल मिल
सुकाउने भट्टी2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.
चाहिने औजार:
हाइड्रोलिक प्रेस
डिस्क थिच्ने डाइ
भर्नियर क्यालिपर3
3
Sinter 1 hour at 1350 °C and furnace-cool
Sinter 1 hour at 1350 °C and furnace-cool
Sinter the discs in air for 1 hour at 1350 °C, then let them cool in the furnace to room temperature (about 15-30 °C).
चाहिने औजार:
मफल भट्टी4
4
Lap to 10 mm by 1.5 mm
Lap to 10 mm by 1.5 mm
Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.
चाहिने औजार:
भर्नियर क्यालिपर5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.
यस चरणका सामग्री:
एल्युमिनियमको ढिक्का1 as required
चाँदीको सुचालक रङ1 as required
तामाको तार2 टुक्राचाहिने औजार:
धातु छर्कने अज्ञात विधि
भर्नियर क्यालिपरसामग्री
6- 9.699 ग्रामप्लेसहोल्डर
- 0.28 ग्रामप्लेसहोल्डर
- 0.021 ग्रामप्लेसहोल्डर
- 1 as requiredप्लेसहोल्डर
- 1 as requiredप्लेसहोल्डर
- 2 टुक्राप्लेसहोल्डर
आवश्यक उपकरणहरू
9- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
सम्बन्धित ब्लुप्रिन्ट
यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।