Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie

Nilikha ni

Charlie

1. Nobyembre 2026DE
5
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)

Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind. Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium. Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
Abantado
1 day

Mga Tagubilin

1

Mix the oxide with lanthanum

Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.

Mga materyales para sa hakbang na ito:

Ytterbium oxideYtterbium oxide1 as required

Mga kailangang kasangkapan:

LantanumLantanum
Crucible na tantalumCrucible na tantalum
2

Reduce in vacuum at 1020 °C

Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.

Mga kailangang kasangkapan:

Induction furnaceInduction furnace
Bombang panghigop ng hanginBombang panghigop ng hangin
Crucible na tantalumCrucible na tantalum
3

Condense the ytterbium at 200-600 °C

Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.

Mga kailangang kasangkapan:

Tantalum na plato ng kondensadorTantalum na plato ng kondensador
4

Melt into ingots under argon

Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.

Mga kailangang kasangkapan:

Crucible na tantalumCrucible na tantalum
Induction furnaceInduction furnace
ArgonArgon

Mga Materyales

1

Mga Kinakailangang Kasangkapan

6

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...