Silicone Sealant: Silicone Oil, Diatomaceous Earth and Methyl Triacetoxysilane (Ceyzeriat 1964)
A one-part silicone that stays a paste in a sealed tube and turns to rubber in the open air. The moisture in the air splits the methyl triacetoxysilane, which then ties the hydroxyl ends of the oil together. Louis Ceyzeriat of Rhône-Poulenc made it with diatomaceous earth as the filler; his Example IV paste became an elastic solid in 15 hours.
Source: L. Ceyzeriat (Rhône-Poulenc), US 3,133,891 (1964), Example IV and columns 3–4. His filler was Celite 350; we use raw diatomaceous earth in its place. Picture drawn by Youblob.
درمیانہ
1 day
ہدایات
1
1
Knead the paste
Knead the paste
Knead 200 parts of hydroxyl-ended silicone oil with 80 parts of diatomaceous earth and 1 part of zinc oxide until it is an even paste. All parts are by weight.
اس مرحلے کے لیے مواد:
ڈائیٹم مٹی80 parts
زنک آکسائیڈ سفوف1 partsدرکار اوزار:
گوندھنے والی مشین
پلڑوں والی ترازو2
2
Drive out all moisture
Drive out all moisture
If the sealant is to be kept, it must be made dry: a paste with zinc oxide especially needs this. Heat it in the mixer at 50–200 °C, stirring, until every trace of moisture is gone, then let it cool. The patent gives that range, not one temperature or time.
درکار اوزار:
گوندھنے والی مشین
گرم پلیٹ
حرارت پیما3
3
Mix in the silane
Mix in the silane
Add 3 parts of methyl triacetoxysilane for every 100 parts of paste: 8.4 parts for the whole 281 parts (our arithmetic). Keep the air out while you mix.
اس مرحلے کے لیے مواد:
میتھائل ٹرائی ایسیٹوکسی سائلین8.4 partsدرکار اوزار:
گوندھنے والی مشین
پلڑوں والی ترازو4
4
Fill dry containers and seal them
Fill dry containers and seal them
Without letting any water in, fill it into dry containers and seal them airtight. Kept like this it stays usable for many months.
درکار اوزار:
ہوا بند ذخیرہ برتن5
5
Use: it cures in the air
Use: it cures in the air
Spread or press it where it is needed and leave it in the air. Ceyzeriat's paste was an elastic solid after 15 hours. Pressed as a 2 mm sheet it tested 25.6 kg/cm² in tension, 290 % stretch and Shore A 50; after 24 hours, 39 kg/cm², 260 % and Shore A 58.
درکار اوزار:
کفگیرمواد
4- 200 partsپلیس ہولڈر
- 80 partsپلیس ہولڈر
- 1 partsپلیس ہولڈر
- 8.4 partsپلیس ہولڈر
یہ بلوپرنٹ بناتا ہے
متعلقہ بلیو پرنٹ
یہ بلیو پرنٹ علم بانٹتے ہیں — تکنیک، مواد یا اصول
Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)
Charlie کی طرف سے
صنعتی
19
0
0
0
0
0

خطرناک
Methyltriacetoxysilane: Methyltrichlorosilane with Acetic Acid, Then Acetic Anhydride
Charlie کی طرف سے
صنعتی
14
0
0
0
0
0

Zinc Oxide (Pharmacy): Zinc Carbonate Precipitated with Hot Soda, Then Heated
Charlie کی طرف سے
غیر نامیاتی
20
0
0
0
0
0
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔