German Harness Leather: Limed, Bated and Bark-Tanned Hides Greased With Linseed Oil and Tallow (Davis, 1885)
Tex

Autor

Tex

14. listopad 2026FO
10
0
0
0
0

German Harness Leather: Limed, Bated and Bark-Tanned Hides Greased With Linseed Oil and Tallow (Davis, 1885)

How German tanners made harness leather, from C. T. Davis's The Manufacture of Leather (1885): green hides soaked, limed twice, unhaired, fleshed and bated, tanned in old liquor and fresh tan with lay-aways until the cut is brown through, split into sides, smoothed, and greased on the flesh side with linseed oil and tallow; then sold brown or blacked with logwood and iron black.
Zaawansowany
Several months

Instrukcje

1

His schedule

Wczytywanie notatnika Jupyter…
2

Read The Manufacture of Leather, ch. XXXI

"Special attention should be paid to this process, as soft leather can only be produced by proper bating, while too much bating is injurious, as it destroys the skin fibres and the grain."
3

Soak and lime

Use green hides if possible. Cut out the horns, soak in running water 6 to 8 hours with frequent rinsing (not longer, or water-stripes form), clean off dung, and lay in weak milk of lime for 24 hours; take out, make fresh lime and replace for 24 hours more, then handle regularly. Salted hides need 3 days' soaking to remove all salt; dried hides are soaked and stretched back to shape.

Materiały do tego kroku:

Skóra surowaSkóra surowa1 sztuka
Wapno gaszoneWapno gaszone1 sztuka

Potrzebne narzędzia:

Kadź garbarskaKadź garbarska
Nóż do skóryNóż do skóry
4

Unhair, flesh and bate

Unhair as soon as the hair pulls out easily, soak a few hours, flesh, soak 24 hours and smooth. Bate for 1 to 3 days by thickness and weather, handling three times a day; neither too little nor too much. Rinse, smooth again, soak several hours and work the flesh side thoroughly with a dull fleshing knife.

Potrzebne narzędzia:

Kobylica do mizdrowaniaKobylica do mizdrowania
Nóż do odmięśnianiaNóż do odmięśniania
Kadź garbarskaKadź garbarska
5

Tan

Lay the hides in old liquor 1 or 2 days. Take them out, ladle out the old tan, add one third of a bushel of fresh tan and replace; the tan is spent in 4 to 8 days, so freshen the vat two or three times more. Then put them in the lay-aways, about as long as sole leather (stout harness leather may need longer). Split a hide after the second layer: uniformly brown through means tanned; pale yellow or white means not.

Materiały do tego kroku:

Kora dębowa (rozdrobniona)Kora dębowa (rozdrobniona)4 sztuk

Potrzebne narzędzia:

Kadź garbarskaKadź garbarska
Nóż do skóryNóż do skóry
6

Split, smooth and grease

Split into sides and number both halves alike. Rinse in old ooze and smooth with a dull fleshing knife on the beam. Choose the best hides for harness. Go over the leather with a fine-edged knife, grease the flesh side with linseed oil and tallow, and hang it up to dry.

Materiały do tego kroku:

Olej lnianyOlej lniany1 sztuka
ŁójŁój1 sztuka

Potrzebne narzędzia:

Kobylica do mizdrowaniaKobylica do mizdrowania
Nóż do odmięśnianiaNóż do odmięśniania
Nóż do skóryNóż do skóry
Pędzel szerokiPędzel szeroki
7

Finish brown or black

Sort into brown and black. Brown is sold as it is or given lustre by glassing. Black is grounded with a decoction of logwood, blacked with iron black and, when nearly dry, pressed.

Materiały do tego kroku:

Zrębki drewna kampeszowegoZrębki drewna kampeszowego1 sztuka

Potrzebne narzędzia:

Pędzel szerokiPędzel szeroki
Duży garnekDuży garnek
8

Troubleshooting

Harness leather troubleshooting.

Flow

Loading...
9

History and honest limits

From Charles Thomas Davis, **The Manufacture of Leather** (Philadelphia, 1885), chapter XXXI (checked on the archive.org scan manufactureoflea01davi, pp. 518-521). He does not give the bate's composition, which tan, or the lime and oil-and-tallow quantities here; oak bark for the tan is our choice. The diagram hero and the tools are ours.

Materiały

6

Wymagane narzędzia

6

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...