Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)
Forge

Autor

Forge

14. listopad 2026NO
8
0
0
0
0

Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)

The first job George Edwinson set his readers in Amateur Work (1886): the smith's rake for the forge fire, which "might be dubbed a poker". A yard of 3/8 in. iron rod drawn to a square then flat point with quarter turns, bent into a crook, and the other end bent round in three heats into a loop handle.
Początkujący
An hour at the forge

Instrukcje

1

His sizes

Wczytywanie notatnika Jupyter…
2

Read Edwinson

"The rake, Fig. 16, might be dubbed a poker, and as this is the most simple tool, we will deal with that first."
3

Light a small fire

Pile slack round the tuyere, scoop a shallow pit in front of it, put in shavings with a few cinders on top, light and blow gently. Draw slack in until the heap glows, then damp the outside so the fire stays within 6 in. (15 cm) of the tuyere.

Materiały do tego kroku:

Węgiel kamienny bitumicznyWęgiel kamienny bitumiczny1 sztuka

Potrzebne narzędzia:

Kuźnia kowalskaKuźnia kowalska
4

Draw the point

Cut 36 in. (91 cm) of 3/8 in. (10 mm) iron rod with a cold chisel. Heat 2 in. of one end glowing white. On the outer edge of the anvil, hammer it lightly on the tip, giving the rod a quarter turn after each blow and drawing it back, to a square point. Strike only while it glows; reheat at a dull red. Next heat, round the corners and draw a flat tapering point (fig. 17).

Materiały do tego kroku:

Pręt z kutego żelazaPręt z kutego żelaza1 sztuka

Potrzebne narzędzia:

Przecinak ślusarskiPrzecinak ślusarski
Kuźnia kowalskaKuźnia kowalska
KowadłoKowadło
MłotekMłotek
5

Crook the end

Heat the point to a dull red and bend it over the outer edge of the anvil with a few light blows into the crook (fig. 16).

Potrzebne narzędzia:

Kuźnia kowalskaKuźnia kowalska
KowadłoKowadło
MłotekMłotek
6

Bend the loop

Heat the rod about 10 in. from the other end to redness and bend it over the anvil edge (fig. 18). Heat 3 in. more of the bent part and shape it (fig. 19). Heat again and bring the end round to touch the shoulder (fig. 20), then shape the loop hot with light blows. (Experienced smiths scarf the end and weld it to the shoulder.)

Potrzebne narzędzia:

Kuźnia kowalskaKuźnia kowalska
KowadłoKowadło
MłotekMłotek
7

Troubleshooting

Rake troubleshooting.

Flow

Loading...
8

History and honest limits

From George Edwinson, "Smithing and Forging" II, **Amateur Work, Illustrated**, vol. V (1886), pp. 211-213 and figs. 15-20 (checked on the archive.org scan amateurworkillus05lond). Metric figures and the tools are ours.

Materiały

2

Wymagane narzędzia

4

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...