Glaze Fit: Crazing, Shivering, and the Mismatch Behind Both
A glazed pot is two materials stuck together that shrink by different amounts as they cool. If the difference is small, the glaze ends up gently squeezed and the pot is stronger for it. If it is large, something has to give.
CRAZING is the glaze cracking into a network of fine lines, because the glaze shrank MORE than the body and is being stretched. SHIVERING is the glaze flaking off in slivers, because it shrank LESS and is being crushed. They are the same problem with opposite signs.
Crazing is often left deliberately, as a decorative crackle. Shivering never is: the flakes are glass, they come off in use, and on anything that holds food that is a genuine hazard rather than a flaw.
Zaawansowany
3 hours
Instrukcje
1
1
Tell them apart, and know which way to move
Tell them apart, and know which way to move
CRAZING looks like a fine web of cracks across the glaze surface, often appearing days or weeks after firing as the body slowly takes up atmospheric moisture and expands. Run a finger over it and it is smooth; the cracks are in the glass, not the surface.
SHIVERING shows as sharp slivers lifting or flaking away, usually at edges, rims and handles where the glaze wraps a curve. It often appears with an audible ping as the kiln cools.
A crazed pot is not waterproof even if it looks it — liquid travels through the cracks into the porous body, which is why a crazed mug eventually smells. That is the practical reason to care beyond appearance.
Materiały do tego kroku:
Szkliwo przezroczyste1 sztuka
Naczynia gliniane suche jak kość1 sztukaPotrzebne narzędzia:
Piec ceramiczny2
2
The numbers behind the mismatch
The numbers behind the mismatch
Wczytywanie notatnika Jupyter…
Materiały do tego kroku:
Szkliwo przezroczyste1 sztuka
Szkliwo ceramiczne1 sztukaPotrzebne narzędzia:
Komputer stacjonarny
Piec ceramiczny3
3
Thickness and edges, before any chemistry
Thickness and edges, before any chemistry
Before changing a recipe, check the application. Glaze that is too thick shivers at edges long before a well-fitted glaze would, because an edge has glaze on two faces meeting at a corner and nothing to hold it.
Wipe glaze thinner on rims, handles and any sharp arris. Rounding sharp edges slightly while the pot is leather-hard also helps a great deal, and costs one pass with a damp sponge.
Most reported glaze-fit faults turn out to be application faults. Chemistry is the answer when the fault persists on properly applied glaze across several firings — which is the change-one-thing-at-a-time rule saving a lot of wasted effort.
Materiały do tego kroku:
Szkliwo przezroczyste1 sztukaPotrzebne narzędzia:
Gąbka
Zestaw narzędzi garncarskich
Suwmiarka cyfrowa 6 cali4
4
Keep test tiles, and label them
Keep test tiles, and label them
Fire test tiles of every glaze on every body you use, with one, two and three dips on the same tile, and keep them. A shelf of tiles answers questions that no amount of reading will.
Mark each tile with the glaze and body before firing — scratched into the clay, not written on with a pen that burns away. An unlabelled test tile is a pretty object of no use whatever.
Record the firing too: which kiln, what schedule, what cone it reached. A glaze is a result of a recipe AND a firing, and the same bucket in a different kiln is a different glaze.
Materiały do tego kroku:
Szkliwo przezroczyste1 sztuka
Glina garncarska niskotopliwa1 kgPotrzebne narzędzia:
Zestaw narzędzi garncarskich
Piec ceramicznyMateriały
4- 4 sztukZastępnik
- 1 sztukaZastępnik
- Szkliwo ceramiczne10% prowizji1 sztukaZastępnik
- Zastępnik
Powiązane blueprinty
Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

Ash Glazing Pottery — The Accidental Discovery That Made Ceramics Waterproof
autor: Clay
RZEMIOSŁO
65
0
0
0
0
0

The States of Clay: Five Conditions, and What Each One Will Let You Do
autor: Clay
Ceramika i glina
24
0
0
0
0
0

One Reading Is Not a Measurement: Repeat It, and Look at the Spread
autor: Penny
Inżynieria
27
0
0
0
0
0
CC0 Domena publiczna
Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.
Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.