Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)

A trace of hot potash opens the ring of D4 and strings it into a long, thick chain. Water added a little at a time then cuts the chains back and leaves hydroxyl groups on their ends, which is what later lets the oil cure into rubber. This is Louis Ceyzeriat's oil A, the base of every sealant in his patent: 21,000 centistokes, 0.15 % hydroxyl. Source: L. Ceyzeriat (Rhône-Poulenc), US 3,133,891 (1964), column 4. His neutraliser was the precipitated silica Hi-Sil X303; we use our precipitated silica in its place. The potash mix and the equipment are ours. Picture drawn by Youblob.
Zaawansowany
2 days

Instrukcje

1

Make the 10 % potash

Dissolve 0.5 part of potassium hydroxide in 4.5 parts of water (our arithmetic for 5 parts of a 10 % solution). All parts are by weight.

Materiały do tego kroku:

Wodorotlenek potasuWodorotlenek potasu0.5 parts
WodaWoda4.5 parts

Potrzebne narzędzia:

Naczynie szklaneNaczynie szklane
Waga szalkowaWaga szalkowa
2

Heat D4 with the potash under nitrogen

Heat 5000 parts of octamethylcyclotetrasiloxane (it melts at 17.5 °C) with the 5 parts of 10 % potash at 150 °C for 3½ hours under nitrogen. The oil thickens to 31,000 centistokes while hot.

Materiały do tego kroku:

Oktametylocyklotetrasiloksan (D4)Oktametylocyklotetrasiloksan (D4)5000 parts

Potrzebne narzędzia:

Szklana kolba destylacyjnaSzklana kolba destylacyjna
Płyta grzejnaPłyta grzejna
TermometrTermometr
MieszadłoMieszadło
Butla z azotemButla z azotem
3

Add water a little at a time

Still hot, add 16.5 parts of water in small portions over 3 hours 40 minutes. The hot oil thins to 1730 centistokes.

Materiały do tego kroku:

WodaWoda16.5 parts

Potrzebne narzędzia:

Szklana kolba destylacyjnaSzklana kolba destylacyjna
Płyta grzejnaPłyta grzejna
TermometrTermometr
MieszadłoMieszadło
4

Cool, then neutralise with silica

Let it cool for 15 hours. Then stir in 50 parts of precipitated silica to neutralise the potash. The liquid now measures 13,400 centistokes at 25 °C.

Materiały do tego kroku:

Krzemionka strącanaKrzemionka strącana50 parts

Potrzebne narzędzia:

Szklana kolba destylacyjnaSzklana kolba destylacyjna
MieszadłoMieszadło
5

Strip the volatiles at 195–200 °C

Heat it to about 195–200 °C in a current of nitrogen, with a water condenser on the outlet. 655 parts of liquid distil over; 4345 parts of oil A stay in the boiler, 21,000 centistokes at 25 °C with 0.15 % hydroxyl groups.

Potrzebne narzędzia:

Szklana kolba destylacyjnaSzklana kolba destylacyjna
Wężownica skraplaczaWężownica skraplacza
Płyta grzejnaPłyta grzejna
TermometrTermometr
Butla z azotemButla z azotem
Słoiki szklane z pokrywkamiSłoiki szklane z pokrywkami

Materiały

4

Wymagane narzędzia

9

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...