Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)

A soft ferrite ring core of magnesium-zinc ferrite: magnesia, zinc oxide and iron oxide ground for a whole day, pressed into a ring and fired at 1400 °C in oxygen. Snoek's ring had an initial permeability of 670 and a Curie point near 100 °C. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example II. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Hejuru
2 days

Amabwiriza

1

Weigh 25.5 : 25.5 : 49 mol %

Mix 25½ mol % pure magnesia, 25½ mol % pure zinc oxide and 49 mol % pure violet iron oxide. Ours, by weight: 9.4 g magnesium oxide, 18.99 g zinc oxide and 71.61 g iron oxide per 100 g. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Ibikoresho by'iyi ntambwe:

Okiside ya magnesiyumuOkiside ya magnesiyumu9.4 g
Ifu ya oxide ya zinkiIfu ya oxide ya zinki18.99 g
Okiside y’icyuma y’ibara ry’isineOkiside y’icyuma y’ibara ry’isine71.61 g

Ibikoresho bikenewe:

Umunzani w'ibiroUmunzani w'ibiro
Agapfukamunwa k'UmukunguguAgapfukamunwa k'Umukungugu
2

Grind for one day in an iron ball mill

Grind the mixture for one day in a mill with iron balls.

Ibikoresho bikenewe:

Urusyo rw'imipira y'icyumaUrusyo rw'imipira y'icyuma
Agapfukamunwa k'UmukunguguAgapfukamunwa k'Umukungugu
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Ibikoresho bikenewe:

Imashini ikanda ikoresha amaziImashini ikanda ikoresha amazi
Ibumbano ryo gukanda impetaIbumbano ryo gukanda impeta
Agapfukamunwa k'UmukunguguAgapfukamunwa k'Umukungugu
4

Fire 1 hour at 1400 °C, cool slowly in oxygen

Heat the ring in oxygen for 1 hour at 1400 °C, then cool it slowly in oxygen. Snoek's ring had an initial permeability of 670 at room temperature and 2 kHz.

Ibikoresho bikenewe:

Itanura ry'umuyoboroItanura ry'umuyoboro
OgisijeneOgisijene
Ibariro rya gazi ifite igitutuIbariro rya gazi ifite igitutu
PirometeroPirometero
Amakoro y'Icyombo GishongeshaAmakoro y'Icyombo Gishongesha
Uturindantoki twihanganira ubushyuheUturindantoki twihanganira ubushyuhe

Ibikoresho

3

Ibikoresho bikenewe

11

CC0 Umurenge rusange

Iyi blueprint yasohowe munsi ya CC0. Ushobora gukoporora, guhindura, gukwirakwiza no gukoresha nta kwemererwa.

Shyigikira Umuremyi ugura ibicuruzwa binyuze muri Blueprint ye Komisiyo y'Umuremyi byashyizweho n'Abacuruzi, cyangwa kora verisiyo nshya y'iyi Blueprint ukayinjiza nk'isano muri Blueprint yawe kugira ngo musangire inyungu.

Ibiganiro

(0)

Injira kugira ngo ujye mu biganiro

Gutegura ibitekerezo...