Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Yaremwe na

Tex

18. Ukwakira 2026FO
7
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Hejuru
1 day

Amabwiriza

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Ibikoresho by'iyi ntambwe:

Utubuye twa polipropileniUtubuye twa polipropileni500 g

Ibikoresho bikenewe:

Imashini isohora pulasitikiImashini isohora pulasitiki
Isahani yo kuboha ubudodoIsahani yo kuboha ubudodo
PirometeroPirometero
Umunzani w'ibiroUmunzani w'ibiro
Uturindantoki tw'UruhuUturindantoki tw'Uruhu
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Ibikoresho bikenewe:

Igikandamiza umwukaIgikandamiza umwuka
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Ibikoresho bikenewe:

Umuyoboro w'umwuka wo kuramburaUmuyoboro w'umwuka wo kurambura
Igikandamiza umwukaIgikandamiza umwuka
Igipima UmuvudukoIgipima Umuvuduko
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Ibikoresho bikenewe:

Igikoresho cyuzuza umuriro hakoreshejwe coronaIgikoresho cyuzuza umuriro hakoreshejwe corona
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Ibikoresho bikenewe:

Ameza yo gutondekahoAmeza yo gutondekaho
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Ibikoresho bikenewe:

Umunzani w'ibiroUmunzani w'ibiro

Ibikoresho

1

Ibikoresho bikenewe

10

CC0 Umurenge rusange

Iyi blueprint yasohowe munsi ya CC0. Ushobora gukoporora, guhindura, gukwirakwiza no gukoresha nta kwemererwa.

Shyigikira Umuremyi ugura ibicuruzwa binyuze muri Blueprint ye Komisiyo y'Umuremyi byashyizweho n'Abacuruzi, cyangwa kora verisiyo nshya y'iyi Blueprint ukayinjiza nk'isano muri Blueprint yawe kugira ngo musangire inyungu.

Ibiganiro

(0)

Injira kugira ngo ujye mu biganiro

Gutegura ibitekerezo...