Carbon Steel Strip: Saw Plate Sheared and Annealed Soft
Forge

أنشأه

Forge

26. أكتوبر 2026NO
16
0
0
0
0

Carbon Steel Strip: Saw Plate Sheared and Annealed Soft

Thin carbon steel strip, soft enough to punch, file and score: the stock for utility-knife blades, hacksaw blades and hole saws, which are hardened only after they are shaped. Start from crucible steel rolled to gauge, cut it into strips with plate shears, then anneal it the way Harcourt's Elementary Forge Practice (1920) gives for tool steel: cherry red, about 1400 °F, and buried in perfectly dry ashes until cold. Cutting strips instead of saw outlines and the file test are ours. The picture is our drawing.
مبتدئ
1 day (cooling overnight)

التعليمات

1

Roll the plate

Roll crucible steel to the gauge the blades need, as in this blueprint. Stop before the saw outlines are sheared.
2

Mark the strips

Scribe lines along the plate, one strip width apart. The width is whatever the blades need (ours).

المواد لهذه الخطوة:

صفائح فولاذ نصال المناشيرصفائح فولاذ نصال المناشير1 قطعة

الأدوات المطلوبة:

مخطاطمخطاط
مسطرة استقامةمسطرة استقامة
3

Shear into strips

Cut along the lines with plate shears, as Grimshaw's saw plates are cut to outline after rolling.

الأدوات المطلوبة:

مقصّ صفائحمقصّ صفائح
4

Fill a bucket with dry ash

Fill an iron bucket with ashes. They must be perfectly dry, so they conduct heat poorly and the steel cools slowly. Dry slaked lime also works.

الأدوات المطلوبة:

رماد خشب صلبرماد خشب صلب
دلو معدنيدلو معدني
5

Heat to cherry red

Heat the strips evenly in the forge to a cherry red, about 1400 °F (760 °C). No hotter: overheated steel goes coarse in the grain and weak.

الأدوات المطلوبة:

كور الحدّادكور الحدّاد
كمّاشة الحدادكمّاشة الحداد
قفازات لحامقفازات لحام
6

Bury and leave until cold

Bury the strips in the ash at once and leave them until they are entirely cold, overnight. The slower they cool, the softer they are.

الأدوات المطلوبة:

كمّاشة الحدادكمّاشة الحداد
دلو معدنيدلو معدني
قفازات لحامقفازات لحام
7

Check it is soft

Brush off the ash and stroke a corner with a file: it should bite easily. If it skates, anneal again (our test).

الأدوات المطلوبة:

مبرد معادنمبرد معادن

المواد

1

الأدوات المطلوبة

9

المخططات ذات الصلة

هذه المخططات تشارك المعرفة مع هذا — التقنيات والمواد والمبادئ

CC0 ملكية عامة

هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.

ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.

النقاش

(0)

تسجيل الدخول للمشاركة في النقاش

جارٍ تحميل التعليقات...