Cast Iron Pot: a Kettle Moulded in Loam, Bottom Up (Bolland, The Iron-Founder, 1892)
Forge

أنشأه

Forge

4. نوفمبر 2026NO
14
0
0
0
0

Cast Iron Pot: a Kettle Moulded in Loam, Bottom Up (Bolland, The Iron-Founder, 1892)

How a founder moulds an iron kettle or pot without a pattern: a brick core is built and coated with loam, swept to the inside shape with a turning board; a layer of sand swept on top stands for the metal's thickness; the cope is built over it, and the space the sand stood for is filled with iron. Bolland's example is an 8 ft kettle 1 3/4 in thick; the same steps serve any size. Variable: the size and wall thickness, set by the sweeps. Source: S. Bolland, The Iron-Founder (1892), pp. 180-183. Unknown: the loam mix and drying. Picture: Fig. 161 of the book.
خبير
Unknown

التعليمات

1

Build and sweep the core

Set the core on a foundation plate strong enough to lift it without springing: a plain plate at least 3 in thick, or a ribbed one 2 in thick. Build the core of bricks in open, coarse mud, bricks well apart so air passes, with half-bricks crossing the joints on the top course and a tie-course here and there. Scrape the joints, rub on soft loam and sweep it to shape as you go round; the first sweep also strikes the flange, the guide and the seat for the cope ring. Finish with a skimming coat of the same loam sifted fine. Ours: sand and clay for the loam. Not given: the loam mix, the size.

الأدوات المطلوبة:

مسبوكات الحديد الزهرمسبوكات الحديد الزهر
طوب من طين محروقطوب من طين محروق
رملرمل
طين خام من المكمنطين خام من المكمن
لوح خشبي منشورلوح خشبي منشور
مالج بنّاءمالج بنّاء
أبعاد غير معروفةأبعاد غير معروفة
2

Strike on the thickness

When the loam is hard enough, change to the thickness sweep. Ram fine-sifted old sand at green-sand temper on by hand from the bottom up, sweeping carefully, dampen and slick it, leaving it about 1/16 in clear of the sweep, and press the flange corner sharp with the trowel. Have all the skinning loam ready first; it must be done in one pass. When it is hard, oil it all over and throw on parting sand. Ours: linseed oil.

الأدوات المطلوبة:

رملرمل
زيت بذر الكتانزيت بذر الكتان
مسحوق الفصلمسحوق الفصل
مالج بنّاءمالج بنّاء
3

Build the cope and gates

Set on the cope ring and build the cope over the thickness, best with building rings and packing so it can be bound down under a cross at once. Bed plates on the sand and bind them down with the cross or binders. Put the riser at the top and enough 3/4 in runners round it, in a circle about 30 in across, to fill the mould quickly. The sand thickness stands for the metal. Not given in these pages: lifting the cope to take the thickness off before closing.

الأدوات المطلوبة:

طوب من طين محروقطوب من طين محروق
مسبوكات الحديد الزهرمسبوكات الحديد الزهر
رملرمل
مالج بنّاءمالج بنّاء
4

Vent and pour

Cut two gutters from the centre of the pit to the outside, sloping gently to the centre, and just before casting pour a little iron down to warm the air so the core gas draws off. Do not fill the trench with shavings and wood, which flash and crack the core. Fill the riser basin with soft straw or hay held down by a dry brick, so gas escapes but no rush of air damages the crown. Pour the iron through the runners. Ours: pig iron melted in a cupola.

المواد لهذه الخطوة:

سبائك حديد خامسبائك حديد خام1 the kettle

الأدوات المطلوبة:

قشّقشّ
فرن قبّيفرن قبّي
مِغرفة صبّ المعدنمِغرفة صبّ المعدن

المواد

1

الأدوات المطلوبة

12

CC0 ملكية عامة

هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.

ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.

النقاش

(0)

تسجيل الدخول للمشاركة في النقاش

جارٍ تحميل التعليقات...