Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
1
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)

A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
İleri
2 days

Talimatlar

1

Weigh barium carbonate, chalk and iron oxide

Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Bu adım için malzemeler:

Baryum karbonat (viterit)Baryum karbonat (viterit)15.79 g
Kalsiyum karbonat (tebeşir tozu)Kalsiyum karbonat (tebeşir tozu)2.002 g
Ferrik oksitFerrik oksit95.55 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Lastik eldivenLastik eldiven
P100 Solunum MaskesiP100 Solunum Maskesi
2

Mill, presinter and mill as in Example 18

As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Etanol - laboratuvar kalitesi, %95Etanol - laboratuvar kalitesi, %95
Kurutma fırınıKurutma fırını
Mufla fırınMufla fırın
Kapaklı kroze (porselen)Kapaklı kroze (porselen)
Pota MaşasıPota Maşası
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).

Gerekli aletler:

Hidrolik presHidrolik pres
Disk presleme kalıbıDisk presleme kalıbı
4

Pass through a 1290 °C zone in 5 minutes

Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.

Gerekli aletler:

Tüp FırınTüp Fırın
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Gerekli aletler:

ElektromıknatısElektromıknatıs
PusulaPusula

Malzemeler

3

Gerekli Aletler

15

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...