Ferrite Toroid Core: Copper-Zinc Ferrite by the Wet Process, Precipitated with Caustic Soda (Snoek 1948)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
6
0
0
0
0

Ferrite Toroid Core: Copper-Zinc Ferrite by the Wet Process, Precipitated with Caustic Soda (Snoek 1948)

Snoek's copper-zinc ferrite made the wet way: copper, zinc and iron salts thrown down together with hot caustic soda, so the particles are very fine and pure. The washed deposit is pre-heated, pressed into a ring and fired in oxygen, with a 30-hour hold at 600 °C. His core reached an initial permeability of 500. Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example II, wet process. Picture: our diagram.
İleri
3 days

Talimatlar

1

Dissolve the copper, zinc and iron salts

Make 1 litre of a purified solution of 0.2 mol copper sulphate, 0.3 mol zinc sulphate and 1 mol iron nitrate. Ours: 49.94 g copper sulphate pentahydrate; weigh the zinc sulphate and ferric nitrate for the hydrate you have.

Bu adım için malzemeler:

Bakır sülfat pentahidrat (CuSO4·5H2O)Bakır sülfat pentahidrat (CuSO4·5H2O)49.94 g
Çinko sülfatÇinko sülfat0.3 mol
Demir(III) nitratDemir(III) nitrat1 mol
Damıtılmış SuDamıtılmış Su1 l

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Borosilikat BeherBorosilikat Beher
Lastik eldivenLastik eldiven
2

Precipitate hot with 9 M caustic soda

Heat the solution and precipitate it with 0.5 litre of 9 molar caustic soda. Ours: 180 g sodium hydroxide in water to 0.5 litre. Strong alkali: goggles and gloves.

Bu adım için malzemeler:

Sodyum Hidroksit — Laboratuvar SaflığıSodyum Hidroksit — Laboratuvar Saflığı180 g

Gerekli aletler:

Borosilikat BeherBorosilikat Beher
Isıtıcı TablaIsıtıcı Tabla
Kimyasal Sıçrama GözlüğüKimyasal Sıçrama Gözlüğü
Lastik eldivenLastik eldiven
3

Wash, dry and pre-heat at 700 °C

Wash out the deposit, dry it, and pre-heat it at 700 °C so it moulds better.

Gerekli aletler:

Süzgeç KâğıdıSüzgeç Kâğıdı
Damıtılmış SuDamıtılmış Su
Kurutma fırınıKurutma fırını
Tüp FırınTüp Fırın
Kapaklı kroze (porselen)Kapaklı kroze (porselen)
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
4

Mould a ring at 4 tons per cm²

Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Gerekli aletler:

Hidrolik presHidrolik pres
Halka Presleme KalıbıHalka Presleme Kalıbı
Toz MaskesiToz Maskesi
5

Heat 3 hours at 900 °C, cool to 600 °C, hold 30 hours

Heat the ring for about 3 hours at 900 °C, cool it to 600 °C at 5 °C per minute, hold it there for 30 hours and let it cool to room temperature, all in a current of oxygen. Snoek's core: initial permeability 500.

Gerekli aletler:

Tüp FırınTüp Fırın
OksijenOksijen
Basınçlı gaz tüpüBasınçlı gaz tüpü
PirometrePirometre
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven

Malzemeler

5

Gerekli Aletler

18

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...