PET Resin: Terephthalic Acid and Ethylene Glycol, Whinfield and Dickson
Charlie

Oluşturan

Charlie

19. Ekim 2026DE
10
0
0
0
0

PET Resin: Terephthalic Acid and Ethylene Glycol, Whinfield and Dickson

PET (polyethylene terephthalate) was invented by Whinfield and Dickson, whose patent (US 2,465,319, 1949) gives this first example: boil terephthalic acid in ethylene glycol until it dissolves, wash and dry the glycol ester, then heat it at 280 °C under nitrogen until it is a viscous polymer that melts at 254–255 °C and can be drawn into fibre. The melt is extruded and cut into chips (pellets) for moulding and spinning. The picture: our diagram.
İleri
About 4 days

Talimatlar

1

Boil the acid in glycol

Reflux 50 g terephthalic acid with 89 g ethylene glycol for about 72 hours, until it has all dissolved. This makes glycol terephthalate.

Bu adım için malzemeler:

Tereftalik AsitTereftalik Asit50 g
Etilen glikolEtilen glikol89 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Yuvarlak dipli balonYuvarlak dipli balon
Yoğuşturucu serpantiniYoğuşturucu serpantini
Isıtıcı TablaIsıtıcı Tabla
2

Wash and dry the ester

Wash the glycol terephthalate with water and dry it under vacuum.

Gerekli aletler:

Damıtılmış SuDamıtılmış Su
Saplı Cam HuniSaplı Cam Huni
Süzgeç KâğıdıSüzgeç Kâğıdı
Vakum pompasıVakum pompası
3

Heat at 280 °C under nitrogen

Melt it and heat at 280 °C for 8½ hours in a slow stream of nitrogen: no air may reach it. It grows thick as it polymerises.

Gerekli aletler:

Yuvarlak dipli balonYuvarlak dipli balon
Isıtıcı TablaIsıtıcı Tabla
Göstergeli ısıl çiftGöstergeli ısıl çift
Azot Gazı TüpüAzot Gazı Tüpü
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
Kimyasal Sıçrama GözlüğüKimyasal Sıçrama Gözlüğü
4

Test for cold-drawing

Pull a thread from the melt with a rod and let it cool. It is ready when the cold thread can be stretched to several times its length. The finished polymer melts at 254–255 °C.

Gerekli aletler:

Cam Karıştırma ÇubuğuCam Karıştırma Çubuğu
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
5

Extrude and cut into chips

Extrude the molten polymer, let it cool, and cut it into chips (pellets).

Gerekli aletler:

Plastik ekstrüderiPlastik ekstrüderi
PeletleyiciPeletleyici
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven

Malzemeler

2

Gerekli Aletler

15

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...