PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
3
0
0
0
0

PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)

A PTFE dispersion is stable on the shelf, but stirred hard enough it curdles. Fifty seconds at 1000 rpm in a baffled beaker and the polymer floats up as a dry-looking, unwettable crumb. Washed and dried, it is a free-flowing powder for rolling into tape, or for cold lubricated extrusion. Source: J. F. Lontz (du Pont), US 2,593,583 (1952), Example 1. Lontz started from a dispersion made with disuccinic acid peroxide; ours is Berry's persulfate dispersion, diluted to his 17 %. Picture drawn by Youblob.
Orta
1 day

Talimatlar

1

Dilute the dispersion to 17 %

Ours: stir the 34 % dispersion with an equal weight of distilled water to get 17 % solids, the strength Lontz used.

Bu adım için malzemeler:

Sulu PTFE dispersiyonuSulu PTFE dispersiyonu1 part
Damıtılmış SuDamıtılmış Su1 part

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Kapaklı Cam KavanozlarKapaklı Cam Kavanozlar
2

Set up the baffled beaker

A 1-gallon stainless beaker, 6.5 in across and 7.5 in deep, with four baffles about ⅜ × 1 in hanging from the cover to within 3 in of the bottom. Stirrer: open turbine, 4 blades 1½ in high, 5 in across, reaching to within 1 in of the bottom.

Gerekli aletler:

Şaşırtmalı karıştırma tankıŞaşırtmalı karıştırma tankı
KarıştırıcıKarıştırıcı
3

Stir hard at 176 °F for 50 seconds

Put in half a gallon of the 17 % dispersion and heat it to 176 °F (80 °C). Run the stirrer at 1000 rpm for 50 seconds (Lontz measured 0.72 hp per gallon). The polymer coagulates and floats, unwetted, on top.

Gerekli aletler:

Şaşırtmalı karıştırma tankıŞaşırtmalı karıştırma tankı
KarıştırıcıKarıştırıcı
Isıtıcı TablaIsıtıcı Tabla
TermometreTermometre
4

Wash hot, then cold

Pour off the water. Wash the polymer with hot water at 176 °F, then with cold water at 60 °F (16 °C), and drain.

Gerekli aletler:

Şaşırtmalı karıştırma tankıŞaşırtmalı karıştırma tankı
TermometreTermometre
5

Dry at 230 °F for 16 hours

Spread the wet polymer on a 100-mesh screen and dry it in an oven at 230 °F (110 °C) for 16 hours. It comes out a free-flowing granular powder that passes 6–8 mesh.

Gerekli aletler:

İnce tel örgülü elekİnce tel örgülü elek
Kurutma fırınıKurutma fırını
Kapaklı Cam KavanozlarKapaklı Cam Kavanozlar

Malzemeler

2

Gerekli Aletler

8

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...