Neodymium Magnets: Nd-Fe-B Alloy Milled, Pressed in a Field and Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. Their sample 5, 79 % iron, 6 % boron and 15 % neodymium by atoms, reached 36.5 MGOe, higher than the best samarium-cobalt magnets of the day.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made; the patent does not say. The magnetising is ours, after Przybylski et al., Sensors 16:569 (2016). The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Uzman
2 days
Talimatlar
1
1
Weigh sample 5: 79 Fe, 6 B, 15 Nd
Weigh sample 5: 79 Fe, 6 B, 15 Nd
Sample 5 is 79 % iron, 6 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 626.8 g iron, 50.4 g ferroboron, 325.8 g neodymium. Unknown: how these three are made.
Bu adım için malzemeler:
Elektrolitik demir626.8 g
Ferrobor50.4 g
Neodimyum metali325.8 gGerekli aletler:
Eşit kollu terazi2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Gerekli aletler:
İndüksiyon fırını
Ateş Kili Potası
Argon
Basınçlı gaz tüpü
Su soğutmalı bakır kalıp
Isıya Dayanıklı Eldiven3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Gerekli aletler:
Dövme Değirmeni
Elek takımı (kademeli göz)
Demir Bilyalı Değirmen
Koruyucu gözlük4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Gerekli aletler:
Manyetik alanlı pres5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 5 measured 13.0 kG remanence, 8.0 kOe coercivity and 36.5 MGOe.
Gerekli aletler:
Tüp Fırın
Argon
Basınçlı gaz tüpü
Isıya Dayanıklı Eldiven6
6
Magnetise the magnets
Magnetise the magnets
Ours, after Przybylski et al., Sensors 16:569 (2016): put each magnet in the coil of an impulse magnetiser and discharge a capacitor bank through it. They found a field of 1200 kA/m enough to saturate N38 sintered Nd-Fe-B; their magnetiser used a 1 mF bank charged up to 5000 V, a thyristor switch and a 440-turn coil of 3 mm copper wire with an 80 mm bore.
Gerekli aletler:
MıknatıslayıcıMalzemeler
3- 626.8 gYer Tutucu
- 50.4 gYer Tutucu
- 325.8 gYer Tutucu
Gerekli Aletler
14- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.