Neodymium Magnets, Sample 12: 55Fe-30B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 12, 55 % iron, 30 % boron and 15 % neodymium by atoms: 4.0 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Uzman
2 days
Talimatlar
1
1
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Sample 12 is 55 % iron, 30 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 328.1 g iron, 301.0 g ferroboron, 389.2 g neodymium. Unknown: how these three are made.
Bu adım için malzemeler:
Elektrolitik demir328.1 g
Ferrobor301 g
Neodimyum metali389.2 gGerekli aletler:
Eşit kollu terazi2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Gerekli aletler:
İndüksiyon fırını
Ateş Kili Potası
Argon
Basınçlı gaz tüpü
Su soğutmalı bakır kalıp
Isıya Dayanıklı Eldiven3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Gerekli aletler:
Dövme Değirmeni
Elek takımı (kademeli göz)
Demir Bilyalı Değirmen
Koruyucu gözlük4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Gerekli aletler:
Manyetik alanlı pres5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 12 measured 4.2 kG remanence, 10.7 kOe coercivity and 4.0 MGOe.
Gerekli aletler:
Tüp Fırın
Argon
Basınçlı gaz tüpü
Isıya Dayanıklı Eldiven6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Gerekli aletler:
Bilinmeyen mıknatıslama yöntemiMalzemeler
3- 328.1 gYer Tutucu
- 301 gYer Tutucu
- 389.2 gYer Tutucu
Gerekli Aletler
14- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.