Neodymium Magnets, Sample 22: 73Fe-8B-19Nd Sintered (Sagawa 1988)
Forge

Oluşturan

Forge

28. Ekim 2026NO
7
0
0
0
0

Neodymium Magnets, Sample 22: 73Fe-8B-19Nd Sintered (Sagawa 1988)

Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 22, 73 % iron, 8 % boron and 19 % neodymium by atoms: 28.0 MGOe. Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Uzman
2 days

Talimatlar

1

Weigh sample 22: 73 Fe, 8 B, 19 Nd

Sample 22 is 73 % iron, 8 % boron and 19 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 542.3 g iron, 64.6 g ferroboron, 397.0 g neodymium. Unknown: how these three are made.

Bu adım için malzemeler:

Elektrolitik demirElektrolitik demir542.3 g
FerroborFerrobor64.6 g
Neodimyum metaliNeodimyum metali397 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
2

Melt by high frequency in argon and cast

Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.

Gerekli aletler:

İndüksiyon fırınıİndüksiyon fırını
Ateş Kili PotasıAteş Kili Potası
ArgonArgon
Basınçlı gaz tüpüBasınçlı gaz tüpü
Su soğutmalı bakır kalıpSu soğutmalı bakır kalıp
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
3

Stamp to 35 mesh, ball-mill to 3-10 µm

Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.

Gerekli aletler:

Dövme DeğirmeniDövme Değirmeni
Elek takımı (kademeli göz)Elek takımı (kademeli göz)
Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Koruyucu gözlükKoruyucu gözlük
4

Press in a 10 kOe field at 1.5 t/cm²

Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.

Gerekli aletler:

Manyetik alanlı presManyetik alanlı pres
5

Sinter in argon at 1000-1200 °C

Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 22 measured 10.9 kG remanence, 11.4 kOe coercivity and 28.0 MGOe.

Gerekli aletler:

Tüp FırınTüp Fırın
ArgonArgon
Basınçlı gaz tüpüBasınçlı gaz tüpü
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
6

Magnetise the magnets

Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.

Gerekli aletler:

Bilinmeyen mıknatıslama yöntemiBilinmeyen mıknatıslama yöntemi

Malzemeler

3

Gerekli Aletler

14

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...