Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
1
0
0
0
0

Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)

A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1200 °C, where his rod held 1,340 gauss with a coercive force of 3,900 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
İleri
2 days

Talimatlar

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.

Bu adım için malzemeler:

Stronsiyum karbonatStronsiyum karbonat29.5 g
Ferrik oksitFerrik oksit191.7 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Lastik eldivenLastik eldiven
P100 Solunum MaskesiP100 Solunum Maskesi
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Etanol - laboratuvar kalitesi, %95Etanol - laboratuvar kalitesi, %95
Kurutma fırınıKurutma fırını
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Gerekli aletler:

Mufla fırınMufla fırın
Kapaklı kroze (porselen)Kapaklı kroze (porselen)
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Etanol - laboratuvar kalitesi, %95Etanol - laboratuvar kalitesi, %95
Kurutma fırınıKurutma fırını
P100 Solunum MaskesiP100 Solunum Maskesi
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Gerekli aletler:

Hidrolik presHidrolik pres
Disk presleme kalıbıDisk presleme kalıbı
6

Sinter 4 hours at 1200 °C

Sinter the discs for 4 hours at 1200 °C in oxygen or in air. The patent's strontium rod at 1200 °C: 1,340 gauss and 3,900 oersted.

Gerekli aletler:

Mufla fırınMufla fırın
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Gerekli aletler:

ElektromıknatısElektromıknatıs
PusulaPusula

Malzemeler

2

Gerekli Aletler

14

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...