Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)

A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1350 °C and fired with the paste at 800 °C, the disc measured a C-value of 90 at 1 mA and a nonlinearity exponent n of 7.3. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
İleri
2 days

Talimatlar

1

Press pure zinc oxide at 340 kg/cm²

Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.

Bu adım için malzemeler:

Çinko Oksit TozuÇinko Oksit Tozu1 as required

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Hidrolik presHidrolik pres
Disk presleme kalıbıDisk presleme kalıbı
KumpasKumpas
2

Sinter 1 hour at 1350 °C and cool

Heat the pressed disc for 1 hour at 1350 °C, then let it cool to room temperature.

Gerekli aletler:

Mufla fırınMufla fırın
3

Lap both faces

Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.

Gerekli aletler:

Silisyum karbür tanesiSilisyum karbür tanesi
KumpasKumpas
4

Coat with bismuth oxide paste and fire at 800 °C

Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.

Bu adım için malzemeler:

Bizmut oksitBizmut oksit1 as required

Gerekli aletler:

Epoksi reçineEpoksi reçine
n-Butanoln-Butanol
Mufla fırınMufla fırın
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.

Bu adım için malzemeler:

Alüminyum külçeAlüminyum külçe1 as required
Gümüş iletken boyaGümüş iletken boya1 as required
Bakır TelBakır Tel2 adet

Gerekli aletler:

Bilinmeyen metal püskürtme yöntemiBilinmeyen metal püskürtme yöntemi
KumpasKumpas

Malzemeler

5

Gerekli Aletler

9

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...