Metal Oxide Varistor: Pure Zinc Oxide at 1400 °C, Bismuth Oxide Paste Fired at 800 °C (Masuyama 1972, Ex. 4)
A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1400 °C and fired with the paste at 800 °C, the disc measured a C-value of 85 at 1 mA and a nonlinearity exponent n of 7.2. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
İleri
2 days
Talimatlar
1
1
Press pure zinc oxide at 340 kg/cm²
Press pure zinc oxide at 340 kg/cm²
Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.
Bu adım için malzemeler:
Çinko Oksit Tozu1 as requiredGerekli aletler:
Eşit kollu terazi
Hidrolik pres
Disk presleme kalıbı
Kumpas2
2
Sinter 1 hour at 1400 °C and cool
Sinter 1 hour at 1400 °C and cool
Heat the pressed disc for 1 hour at 1400 °C, then let it cool to room temperature.
Gerekli aletler:
Mufla fırın3
3
Lap both faces
Lap both faces
Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.
Gerekli aletler:
Kumpas4
4
Coat with bismuth oxide paste and fire at 800 °C
Coat with bismuth oxide paste and fire at 800 °C
Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 800 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.
Bu adım için malzemeler:
Bizmut oksit1 as requiredGerekli aletler:
Epoksi reçine
n-Butanol
Mufla fırın5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.
Bu adım için malzemeler:
Alüminyum külçe1 as required
Gümüş iletken boya1 as required
Bakır Tel2 adetGerekli aletler:
Bilinmeyen metal püskürtme yöntemi
KumpasMalzemeler
5- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
- 2 adetYer Tutucu
Gerekli Aletler
9- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.