Forged Flat Drills: Tool Steel Drawn to Blade and Square Taper Head, Tempered by Colour for the Metal to Be Drilled (Edwinson, 1886)
How a smith forged his own set of flat drills, from George Edwinson's series in Amateur Work (1886): 3/4 in. square tool steel drawn to a blade and shank with a square taper head, hardened in 45-50 F water and tempered by watching the colours run from a red-hot iron (pale straw for cast iron, orange yellow for wrought iron and copper, purplish yellow for wood), then ground to a notched gauge with clear corners.
Advanced
An hour or two per drill
Instructions
1
1
His sizes
His sizes
Loading Jupyter Notebook...
2
2
Read Edwinson
Read Edwinson
"A good drill may be made to turn out good work even when all other parts are indifferently made."
3
3
Draw the blade
Draw the blade
Cut a two-foot length of 3/4 in. (19 mm) square tool steel. Heat 3 in. to blood red in a clean fire, never hotter, and hammer only down to a dull red before reheating. Draw out the blade and shank first (fig. 61), close to shape.
Materials for this step:
Tool Steel Bar1 pieceTools needed:
Blacksmith Forge
Anvil
Hammer
Blacksmith Tongs4
4
Forge the head
Forge the head
Cut off the length for the head, hold the blade and shank in grooved flat-bit tongs, and forge a square taper head to fit your brace socket, sides equal, shank and blade central. Finish at a dull red, set true, cool.
Tools needed:
Hot Chisel
Blacksmith Forge
Anvil
Hammer
Blacksmith Tongs5
5
Shape and substance
Shape and substance
Taper gradually from head to shank, keep the shank even for an inch or two, then let the blade swell out and thin toward the point (figs. 62, 63). Blade about 1/16 in. at the point and 1/8 in. at the corners for a 1/4 in. drill, up to 3/16 in. for 1/2 or 3/4 in.; a 1/4 in. drill's shank half as thick as a 1/2 in. blade. Leave blades a little full for grinding.
Tools needed:
Blacksmith Forge
Anvil
Hammer6
6
Harden
Harden
Heat to red and plunge the drill straight down into cool water of 45-50 F (7-10 C), holding it until cold: icy water makes the edges brittle. Brighten the blade and part of the shank on a brick or grit-stone.
Materials for this step:
Water1 pieceTools needed:
Blacksmith Forge
Bucket
Thermometer
Whetstone7
7
Temper by colour
Temper by colour
Lay the shank across a red-hot piece of stout iron and watch the tints run toward the blade: straw, yellow, orange yellow, purplish yellow, purple, blues. For cast iron and hard brass stop when pale straw reaches the blade, dipping the blade to hold the later colours back while the shank cools in air. For wrought iron, soft steel or copper let the blade reach orange yellow. For wood only, let blade and shank reach purplish yellow and cool slowly.
Materials for this step:
Water1 pieceTools needed:
Blacksmith Forge
Iron Plate
Bucket8
8
Grind to a gauge
Grind to a gauge
Cut gauges from thin sheet brass with notches at the point angles (figs. 65, 66): very obtuse for cast iron and hard brass, more acute for wrought iron, tough steel and copper. Grind both edges equal with the point on the centre line, and give the corners clearance (fig. 70). Grind each blade to its finished size.
Materials for this step:
Brass Sheet1 pieceTools needed:
Files (Hand File)
Grindstone9
9
Troubleshooting
Troubleshooting
Drill troubleshooting.
Flow
Loading...
10
10
History and honest limits
History and honest limits
From George Edwinson, "Smithing and Forging" IV, **Amateur Work, Illustrated**, vol. V (1886), pp. 348-351 and figs. 54-70 (checked on the archive.org scan amateurworkillus05lond; the scan reads 3/4 in. bar where the OCR text says 1/2). He also hardened glass and china drills in mercury: left out here (mercury is a poison). Metric figures, the brass gauge stock and the thermometer are ours.
Materials
3- 1 piecePlaceholder
- 2 piecesPlaceholder
- 1 piecePlaceholder
This blueprint makes
Related Blueprints
These blueprints share knowledge with this one — techniques, materials, or principles that connect them in the learning graph.

Quench Hardening and Tempering a Steel Blade — Heat Treatment Fundamentals
by Forge
Ancient
98
0
0
0
2
0

Drawing Out: Making It Longer by Making It Thinner
by Forge
Metalworking Tools
52
0
0
0
0
0

Flat-Bit Tongs and the Tongs Made from Them, down to Crucible Tongs: Welded Reins, Riveted Joint (Edwinson, 1886)
by Forge
Metalworking
9
0
0
0
0
0
CC0 Public Domain
This blueprint is released under CC0. You are free to copy, modify, distribute, and use this work for any purpose, without asking permission.
Support the Maker by purchasing products through their Blueprint where they earn a Maker Commission set by Vendors, or create a new iteration of this Blueprint and include it as a connection in your own Blueprint to share revenue.